Compact polyamide Janus membrane distillation membrane as well as preparation method and application thereof

By constructing a PA/PVA or PA/ANF composite layer on a hydrophobic membrane, the permeability and stability of traditional membranes under oil and surfactant pollution are solved, and efficient membrane distillation performance and long-term stability are achieved. It is suitable for Desalination treatment of high-salt wastewater.

CN118874240AActive Publication Date: 2024-11-01SHANDONG UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411299494.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-01
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

When traditional polymer hydrophobic membrane distillation membranes face oil and surfactant contamination, it is difficult to maintain high permeability flux and long-term stability at the same time, and the preparation is complex, which limits the application of membrane distillation technology.

Method used

A dense polyamide Janus film composed of a hydrophilic modified hydrophobic film, a hydrophilic intermediate layer and a polyamide layer is used to form a PA/PVA or PA/ANF composite layer through interfacial polymerization, which enhances the mechanical strength and anti-pollution properties of the film.

Benefits of technology

The stable steam flux and low conductivity permeate in oily and high-salt wastewater are achieved, which extends the service life of the membrane and improves the anti-pollution and wetting properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874240A_ABST
    Figure CN118874240A_ABST
Patent Text Reader

Abstract

The invention provides a compact polyamide Janus membrane distillation membrane as well as a preparation method and application thereof, and belongs to the technical field of membrane preparation. The compact polyamide Janus membrane distillation membrane comprises a hydrophilic modified hydrophobic membrane, a hydrophilic middle layer and a polyamide layer which are sequentially arranged from bottom to top, the hydrophilic middle layer is a polyvinyl alcohol layer or an aramid nanofiber layer, and the hydrophilic middle layer is obtained by uniformly coating the surface of one side of the hydrophilic modified hydrophobic membrane with a hydrophilic middle layer solution. And forming a polyamide layer on the surface of the hydrophilic middle layer by utilizing an interfacial polymerization reaction, thereby obtaining the compact polyamide Janus membrane distillation membrane. A continuous and uniform PVA or ANF hydrophilic middle layer is constructed on a hydrophobic substrate subjected to hydrophilic modification, so that the storage amount of amine monomers in a water phase is increased, a complete interfacial polymerization reaction is promoted, and the obtained polyamide Janus membrane distillation membrane can keep stable steam flux and permeation effluent with very low electric conductivity during long-term continuous operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of membrane preparation, and relates to a dense polyamide Janus membrane distillation membrane and a preparation method and application thereof, and in particular to a dense polyamide Janus membrane distillation membrane based on a polyvinyl alcohol or aramid nanofiber intermediate layer and a preparation method and application thereof. Background Art

[0002] Membrane distillation (MD) is a desalination technology that uses the steam pressure difference on both sides of the membrane as the driving force for mass transfer to allow water vapor to pass through a porous hydrophobic membrane material while intercepting liquids and non-volatile components (such as ions, etc.). MD is a product of the combination of membrane and thermal methods, and combines the advantages of membrane technology and distillation technology. It can achieve nearly 100% removal of salt ions in the solution, and has great advantages in treating high-concentration, highly polluted brine and utilizing low-grade heat such as industrial waste heat, as well as solar energy and geothermal energy. In addition, compared with traditional membrane technology and thermal desalination processes (reverse osmosis technology (RO), forward osmosis (FO), multi-effect distillation (MED), multi-stage flash evaporation (MSF)), MD technology has simple equipment and easy operation, and has the flexibility to build a large-scale production system. Therefore, MD has certain competitiveness and application prospects as a sustainable, low-energy consumption seawater desalination and brine desalination technology. However, traditional polymer hydrophobic MD membranes face serious problems such as membrane fouling and membrane infiltration, which seriously limit the further promotion and application of membrane distillation technology.

[0003] Generally, membrane fouling caused by hydrophobic organic pollutants (such as oil droplets) and membrane wetting caused by amphiphilic organic matter (such as surfactants) greatly limit the applicability of MD, which seriously affects the performance of MD membranes (such as permeability and salt rejection), increases the cleaning frequency, shortens the membrane life, and even causes irreversible membrane damage. In order to solve the above problems, various advanced MD membranes, such as superhydrophobic membranes, fully hydrophobic membranes, and Janus membranes, have been developed by spraying, surface fluorination, and polymer coating methods. However, the current methods still have the following problems: in the case of feed brine containing both oil and surfactant pollutants, the high permeation flux and long-term stability of the membrane cannot be met at the same time; it involves a series of difficult to control and complex procedures, and it is difficult to mass produce and prepare. Therefore, the preparation of a high-performance and easily scalable membrane distillation membrane is a technical problem that technicians in this field urgently need to solve. Summary of the invention

[0004] In order to solve the above technical problems, the present invention proposes a dense polyamide Janus membrane distillation membrane and a preparation method and application thereof.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] One of the technical solutions of the present invention:

[0007] A dense polyamide Janus membrane distillation membrane comprises a hydrophilic modified hydrophobic membrane, a hydrophilic middle layer and a polyamide (PA) layer which are arranged in sequence from bottom to top, wherein the hydrophilic middle layer is a polyvinyl alcohol (PVA) layer or an aramid nanofiber (ANF) layer.

[0008] Furthermore, the hydrophilic-modified hydrophobic membrane includes one of a hydrophilic-modified polytetrafluoroethylene membrane, a polyvinylidene fluoride membrane, a polypropylene membrane and a composite membrane thereof.

[0009] Furthermore, the hydrophilic modification method includes one or any combination of polydopamine deposition, polydopamine / polyethyleneimine deposition, tannic acid / 3-aminopropyltriethoxysilane adhesion, sodium hydroxide solution immersion, and plasma treatment.

[0010] The second technical solution of the present invention:

[0011] A method for preparing the dense polyamide Janus membrane distillation membrane, comprising uniformly coating a hydrophilic intermediate layer solution on one side of a hydrophobic membrane that has been hydrophilically modified to obtain a hydrophilic intermediate layer, and then using an interfacial polymerization reaction to sequentially infiltrate the surface of the hydrophilic intermediate layer with an aqueous phase monomer solution and an oil phase monomer solution to form a polyamide (PA) layer, thereby obtaining the dense polyamide Janus membrane distillation membrane;

[0012] The hydrophilic intermediate layer solution is a polyvinyl alcohol (PVA) solution or an aramid nanofiber (ANF) solution.

[0013] Furthermore, the polyvinyl alcohol solution is obtained by stirring polyvinyl alcohol and deionized water at 90° C. until they are uniformly mixed, and the stirring time is 6-10 hours;

[0014] The aramid nanofiber solution is obtained by dissolving potassium hydroxide in deionized water, then magnetically stirring for 48-96 hours and adding dimethyl sulfoxide and aramid nanofiber.

[0015] Furthermore, the mass concentration of the polyvinyl alcohol solution is 6-12%, the usage ratio of potassium hydroxide to deionized water is 0.5-2 g / mL, the mass ratio of potassium hydroxide to aramid nanofiber is (0.5-2):1, and the usage ratio of aramid nanofiber to dimethyl sulfoxide is 0.01-0.04 g / mL.

[0016] Furthermore, the aqueous monomer solution is a polyamine aqueous solution with a mass concentration of 0.5-2%, and the polyamine is one of piperazine, m-phenylenediamine or polyethyleneimine.

[0017] Furthermore, the oil phase monomer solution is a mixed solution of a polyacyl chloride and an organic solvent, the mass concentration of the polyacyl chloride in the oil phase monomer solution is 0.02-0.3%, the polyacyl chloride is one of trimesoyl chloride, isophthaloyl chloride, cyclohexanetrichloride, cyclopentanetrichloride, propanoyl chloride or glutaryl chloride, and the organic solvent is one of n-hexane, n-heptane, dodecane or tetradecane.

[0018] Furthermore, the coating amount of the hydrophilic intermediate layer solution is 0.01-0.02 mL / cm 2 The amount of the aqueous monomer solution used during infiltration is 0.15-0.25 mL / cm 2 The coating amount of the oil phase monomer solution during infiltration is 0.15-0.25 mL / cm 2 .

[0019] Furthermore, the uniform coating is performed by using a scraper with a gap of 50 microns.

[0020] Furthermore, the following steps are included:

[0021] (1) uniformly coating a hydrophilic intermediate layer solution on one surface of a hydrophilic modified hydrophobic membrane, and obtaining a hydrophilic modified hydrophobic membrane carrying a hydrophilic intermediate layer after drying;

[0022] (2) The hydrophilic modified hydrophobic membrane carrying the hydrophilic intermediate layer is fixed, and then the aqueous phase monomer solution is dripped onto the surface of the hydrophilic intermediate layer for infiltration, and then dried after standing. Thereafter, the oil phase monomer solution is continuously dripped onto the surface for infiltration, and then dried after standing, to obtain the dense polyamide Janus membrane distillation membrane.

[0023] Furthermore, in step (1), the drying is air-drying or drying at 25-35°C.

[0024] Furthermore, in step (2), the standing time after the aqueous monomer solution is added is 3-10 minutes, and the excess aqueous monomer solution is removed, and then the mixture is dried at 30°C for 30 minutes; the standing time after the oil phase monomer solution is added is 1-2 minutes, and the excess oil phase monomer solution is removed, and then the mixture is dried at 60°C for 5-10 minutes.

[0025] The third technical solution of the present invention:

[0026] The application of the dense polyamide Janus membrane distillation membrane in membrane distillation.

[0027] Furthermore, when used, the side of the dense polyamide Janus membrane distillation membrane on which the PA / PVA composite layer or the PA / ANF composite layer is loaded is brought into contact with the feed liquid.

[0028] The reaction principle involved in the technical solution of the present invention is:

[0029] PVA has the advantages of strong film-forming ability, good hydrophilicity and good biocompatibility, and can be used as an antifouling material to prepare high-performance Janus membrane distillation membranes. The present invention uses PVA solution to cast on the surface of a hydrophilic modified hydrophobic membrane, and then through a drying shrinkage-rehydration process, a hydrogel-like PVA intermediate coating is constructed in a simpler and greener way. ANF is derived from Kevlar, which is famous for its excellent mechanical properties, and has a high aspect ratio and symmetrical aromatic rings in the main chain units, which will help enhance the mechanical strength of the Janus membrane distillation membrane. The present invention uses a hydrophilically modified hydrophobic microporous membrane, which is conducive to the loading of the PVA or ANF coating, thereby ensuring the formation of a uniform and hydrophilic intermediate coating on the surface of the hydrophobic membrane.

[0030] The construction of the hydrophilic PVA and ANF intermediate coating increases the storage capacity of amine monomers in the aqueous phase and accelerates the interfacial polymerization reaction, thereby forming a complete and defect-free polyamide (PA) layer. Since the PA-PVA and PA-ANF composite layers are hydrophilic and thin, the flux of the obtained membrane is comparable to that of the unmodified hydrophobic membrane. At the same time, thanks to the formation of a complete and defect-free PA layer on the constructed intermediate layer, the obtained dense polyamide Janus membrane distillation membrane has a stable steam flux and a low conductivity permeate. Therefore, the scalable preparation process and robust membrane distillation performance of the dense polyamide Janus membrane distillation membrane based on the PVA and ANF intermediate layer have great potential in the practicality of desalination of oily and high-salt wastewater.

[0031] Compared with the prior art, the present invention has the following advantages and technical effects:

[0032] The present invention constructs a continuous and uniform PVA or ANF hydrophilic intermediate layer on a hydrophilically modified hydrophobic substrate, and performs interfacial polymerization on this basis. Compared with interfacial polymerization directly on the hydrophobic substrate, the PVA or ANF hydrophilic intermediate layer increases the storage capacity of amine monomers in the water phase and promotes a complete interfacial polymerization reaction, thereby forming a dense and defect-free polyamide Janus membrane distillation membrane, which can maintain a stable steam flux and permeate water with very low conductivity during long-term continuous operation. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0034] Figure 1 is a scanning electron microscope image of the original polytetrafluoroethylene membrane surface of Example 1;

[0035] Figure 2This is a scanning electron microscope image of the dense PA / PVA Janus membrane distillation membrane obtained in Example 1;

[0036] Figure 3 This is a scanning electron microscope image of the dense PA / ANF Janus membrane distillation membrane obtained in Example 2;

[0037] Figure 4 The water contact angle in air and the oil contact angle underwater of the polytetrafluoroethylene membrane and the dense PA / PVA and PA / ANF Janus membrane distillation membranes in Examples 3 and 4;

[0038] Figure 5 The flux and effluent conductivity diagrams of the polytetrafluoroethylene membrane and the dense PA / PVA and PA / ANF Janus membrane distillation membranes in Examples 3 and 4;

[0039] Figure 6 The graphs are the flux and effluent conductivity of the polytetrafluoroethylene membrane in Examples 5 and 6 when treating the feed liquid as an oil-containing salt solution;

[0040] Figure 7 The flux and effluent conductivity diagrams of the dense PA / PVA and PA / ANF Janus membrane distillation membranes in Examples 5 and 6 when treating a feed liquid that is an oil-containing salt solution;

[0041] Figure 8 The graphs are the flux and effluent conductivity of the polytetrafluoroethylene membrane in Examples 5 and 6 when treating a feed liquid that is a salt solution containing a surfactant;

[0042] Fig. 9 The flux and effluent conductivity diagrams of the dense PA / PVA and PA / ANF Janus membrane distillation membranes in Examples 5 and 6 when treating a feed liquid that is a salt solution containing a surfactant;

[0043] Fig.10 The graphs are the flux and effluent conductivity of the polytetrafluoroethylene membrane in Examples 7 and 8 when treating a salt solution of an oil-water emulsion stabilized by a surfactant as the feed liquid;

[0044] Fig.11 Graphs showing the flux and effluent conductivity of the dense PA / PVA and PA / ANF Janus membrane distillation membranes in Examples 7 and 8 when treating a saline solution of an oil-water emulsion stabilized by a surfactant as the feed liquid.

[0045] Fig.12 Graph showing the liquid entry pressure values ​​of the PA / PVA Janus membrane distillation membrane and polytetrafluoroethylene membrane of Example 1, the PA / ANFJanus membrane distillation membrane of Example 2, and the PAJanus membrane distillation membrane of Comparative Example 1. DETAILED DESCRIPTION

[0046] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0047] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0048] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0049] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0050] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0051] An embodiment of the present invention provides a dense polyamide Janus membrane distillation membrane, comprising a hydrophilic-modified hydrophobic membrane, a hydrophilic intermediate layer and a polyamide (PA) layer arranged in sequence from bottom to top, wherein the hydrophilic intermediate layer is a polyvinyl alcohol (PVA) layer or an aramid nanofiber (ANF) layer.

[0052] In a preferred embodiment of the present invention, the hydrophilic-modified hydrophobic membrane comprises one of a hydrophilic-modified polytetrafluoroethylene membrane, a polyvinylidene fluoride membrane, a polypropylene membrane and a composite membrane thereof, preferably a polytetrafluoroethylene membrane.

[0053] The use of hydrophilic modified hydrophobic microporous membranes is beneficial to the loading of PVA and ANF coatings, thereby ensuring the formation of a uniform and hydrophilic intermediate coating on the surface of the hydrophobic membrane. The construction of the hydrophilic PVA and ANF intermediate coatings increases the storage capacity of amine monomers in the aqueous phase and accelerates the interfacial polymerization reaction, thereby forming a complete and defect-free polyamide (PA) layer. Due to the hydrophilicity and thin PA / PVA and PA / ANF composite layers, the flux of the obtained membrane is comparable to that of the unmodified hydrophobic membrane. At the same time, thanks to the complete and defect-free PA layer formed on the intermediate layer, the obtained dense polyamide Janus membrane distillation membrane has a stable vapor flux and a permeate with low conductivity.

[0054] In a preferred embodiment of the present invention, the hydrophilic modification method includes one or any combination of polydopamine deposition, polydopamine / polyethyleneimine deposition, tannic acid / 3-aminopropyltriethoxysilane adhesion, sodium hydroxide solution immersion, and plasma treatment, preferably polydopamine deposition and 3-aminopropyltriethoxysilane adhesion.

[0055] The embodiment of the present invention also provides a method for preparing the dense polyamide Janus membrane distillation membrane, wherein a hydrophilic intermediate layer solution is uniformly coated on one side of a hydrophobic membrane that has been hydrophilically modified to obtain a hydrophilic intermediate layer, and then an aqueous phase monomer solution and an oil phase monomer solution are sequentially de-wetted on the surface of the hydrophilic intermediate layer by an interfacial polymerization reaction to form a polyamide (PA) layer, thereby obtaining the dense polyamide Janus membrane distillation membrane;

[0056] The hydrophilic intermediate layer solution is a polyvinyl alcohol (PVA) solution or an aramid nanofiber (ANF) solution.

[0057] More specifically, the following steps are included:

[0058] (1) uniformly coating the hydrophilic intermediate layer solution on one surface of the hydrophilically modified hydrophobic membrane, and drying (naturally drying or drying at 25-35° C.) to obtain a hydrophilically modified hydrophobic membrane carrying a hydrophilic intermediate layer;

[0059] (2) The hydrophilic modified hydrophobic membrane carrying the hydrophilic intermediate layer is fixed on a membrane mold made of polytetrafluoroethylene material, and then the hydrophilic intermediate layer is uniformly infiltrated with an aqueous monomer solution, allowed to stand for 3-10 minutes and excess aqueous monomer solution is removed, and dried at 30° C. for 30 minutes, and then infiltrated with an oily monomer solution, allowed to stand for 1-2 minutes and excess oily monomer solution is removed, and dried at 60° C. for 5-10 minutes to obtain the dense polyamide Janus membrane distillation membrane.

[0060] In a preferred embodiment of the present invention, the polyvinyl alcohol solution is obtained by stirring polyvinyl alcohol and deionized water at 90° C. until they are uniformly mixed, and the stirring time is 6-10 hours.

[0061] In a preferred embodiment of the present invention, the aramid nanofiber solution is obtained by dissolving potassium hydroxide in deionized water, followed by magnetic stirring for 48-96 hours and adding dimethyl sulfoxide and aramid nanofibers.

[0062] In a preferred embodiment of the present invention, the mass concentration of the polyvinyl alcohol solution is 6-12%, preferably 8-10%.

[0063] In a preferred embodiment of the present invention, the dosage ratio of potassium hydroxide to deionized water is 0.5-2 g / mL, preferably 1 g / mL, the mass ratio of potassium hydroxide to aramid nanofiber is (0.5-2):1, preferably (0.8-1):1, and the dosage ratio of aramid nanofiber to dimethyl sulfoxide is 0.01-0.04 g / mL, preferably 0.02-0.025 g / mL.

[0064] In a preferred embodiment of the present invention, the aqueous monomer solution is a polyamine aqueous solution with a mass concentration of 0.5-2%, and the polyamine is one of piperazine, m-phenylenediamine or polyethyleneimine, preferably a m-phenylenediamine aqueous solution or a piperazine aqueous solution with a mass concentration of 1-2%.

[0065] In a preferred embodiment of the present invention, the oil phase monomer solution is a mixed solution of a polyacyl chloride and an organic solvent, the mass concentration of the polyacyl chloride in the oil phase monomer solution is 0.02-0.3%, preferably 0.02-0.1%, the polyacyl chloride is one of trimesoyl chloride, isophthaloyl chloride, cyclohexanetrichloride, cyclopentanetrichloride, propanetrichloride or glutaryltrichloride, preferably trimesoyl chloride, and the organic solvent is one of n-hexane, n-heptane, dodecane or tetradecane, preferably n-hexane.

[0066] In a preferred embodiment of the present invention, the coating amount of the hydrophilic intermediate layer solution is 0.01-0.02 mL / cm 2 The amount of the aqueous monomer solution used during infiltration is 0.15-0.25 mL / cm 2 The amount of the oil phase monomer solution used during infiltration is 0.15-0.25 mL / cm 2 .

[0067] In a preferred embodiment of the present invention, the uniform coating is performed using a scraper with a gap of 50 microns.

[0068] The embodiment of the present invention also proposes the application of the dense polyamide Janus membrane distillation membrane in membrane distillation.

[0069] When used, the side of the dense polyamide Janus membrane distillation membrane surface loaded with the PA / PVA composite layer or the PA / ANF composite layer is brought into contact with the feed liquid.

[0070] The two sides of the membrane distillation membrane are respectively the feed liquid on the hot side and the permeate on the cold side, wherein the feed liquid is a salt solution, more preferably a salt solution with a surfactant added and an oil-water emulsion stabilized by the surfactant, and the permeate is deionized water.

[0071] The purpose of adding oil to the feed liquid is to test the anti-fouling performance of dense polyamide Janus membrane distillation; the purpose of adding surfactant to the feed liquid is to test the anti-wetting performance of dense polyamide Janus membrane distillation; the purpose of adding surfactant-stabilized oil-water emulsion to the feed liquid is to test the simultaneous anti-fouling and anti-wetting performance of dense polyamide Janus membrane distillation membrane.

[0072] The raw materials used in the embodiments of the present invention are all commercially available.

[0073] The technical solution of the present invention is further illustrated by the following embodiments.

[0074] Example 1

[0075] A dense polyamide Janus membrane distillation membrane comprises a hydrophilic modified hydrophobic membrane, a hydrophilic polyvinyl alcohol (PVA) layer and a polyamide (PA) layer arranged in sequence from bottom to top, and a preparation method comprises the following steps:

[0076] (1) 0.1 g dopamine and 0.1 g polyethyleneimine were dissolved in 50 mmol / L, 50 mL Tris-HCl buffer solution (pH=8) to obtain an activation solution, and then the upper surface of the polytetrafluoroethylene membrane was immersed in the activation solution. After standing for 12 hours, the membrane surface was rinsed and naturally dried to obtain a polytetrafluoroethylene membrane with one side hydrophilically modified;

[0077] (2) 8 g of PVA powder was added to 92 g of deionized water and stirred under magnetic force at 90° C. for 8 h to form a uniform PVA solution. The obtained PVA solution was poured onto one side of the hydrophilically modified polytetrafluoroethylene membrane obtained in step (1) and evenly coated with a scraper with a gap of 50 μm. The coating amount was 0.012 mL / cm 2 , after being evenly coated, it was placed at 35°C and dried for 30 min to obtain a hydrophilic-modified hydrophobic membrane loaded with PVA film;

[0078] (3) dissolving m-phenylenediamine in deionized water and stirring to mix well to obtain an aqueous monomer solution, wherein the concentration of m-phenylenediamine in the aqueous monomer solution is 2 wt %, dissolving trimesoyl chloride in n-hexane and mixing well by ultrasonication to obtain an oily monomer solution, wherein the concentration of trimesoyl chloride in the oily monomer solution is 0.2 wt %;

[0079] (4) The hydrophilic-modified hydrophobic membrane loaded with PVA film prepared in step (2) is fixed on a polytetrafluoroethylene mold, and then the aqueous monomer solution prepared in step (3) is used to uniformly infiltrate the surface of the PVA film, with the amount used being 0.16 mL / cm 2 After standing for 5 minutes, remove the excess aqueous monomer solution, dry naturally, and then continue to use the oil phase monomer solution prepared in step (3) to evenly infiltrate the surface of the substrate. The amount used is 0.16 mL / cm 2 After evenly spreading, let it stand for 2 minutes, remove the excess oil phase monomer solution, and dry it at 60°C for 10 minutes to obtain a dense polyamide Janus membrane distillation membrane, which is recorded as a dense PA / PVA Janus membrane distillation membrane.

[0080] Example 2

[0081] A dense polyamide Janus membrane distillation membrane comprises a hydrophilic-modified hydrophobic membrane, a hydrophilic aramid nanofiber (ANF) layer and a polyamide (PA) layer arranged in sequence from bottom to top, and a preparation method comprises the following steps:

[0082] (1) 0.1 g dopamine and 0.1 g polyethyleneimine were dissolved in 50 mmol / L, 50 mL Tris-HCl buffer solution (pH=8) to obtain an activation solution, and then the upper surface of the polytetrafluoroethylene membrane was immersed in the activation solution. After standing for 12 hours, the membrane surface was rinsed and naturally dried to obtain a polytetrafluoroethylene membrane with one side hydrophilically modified;

[0083] (2) 0.4 g KOH was completely dissolved in 0.4 mL deionized water, and then 20 mL dimethyl sulfoxide and 0.4 g aramid nanofiber were added under magnetic stirring. After stirring at a constant speed for 50 h, a deep red ANF solution was obtained. The obtained ANF solution was poured onto one side of the hydrophilically modified polytetrafluoroethylene membrane prepared in step (1) and evenly coated with a scraper with a gap of 50 μm. The amount of the solution added was 0.02 mL / cm 2 The coated membrane was slowly immersed in deionized water and allowed to stand for 30 min, and then naturally dried to obtain a hydrophilic-modified hydrophobic membrane loaded with ANF membrane;

[0084] (3) dissolving m-phenylenediamine in deionized water and stirring to mix well to obtain an aqueous monomer solution, wherein the concentration of m-phenylenediamine in the aqueous monomer solution is 2 wt %, dissolving trimesoyl chloride in n-hexane and mixing well by ultrasonication to obtain an oily monomer solution, wherein the concentration of trimesoyl chloride in the oily monomer solution is 0.2 wt %;

[0085] (4) The hydrophilic-modified hydrophobic membrane loaded with ANF prepared in step (2) is fixed on a polytetrafluoroethylene membrane, and then the aqueous monomer solution prepared in step (3) is used to evenly infiltrate the surface of the PVA membrane in an amount of 0.16 mL / cm 2 After standing for 5 minutes, remove the excess aqueous monomer solution, dry naturally, and then continue to use the oil phase monomer solution prepared in step (3) to evenly infiltrate the surface of the substrate. The amount used is 0.16 mL / cm 2 After being evenly spread, the mixture was allowed to stand for 2 minutes, the excess oil phase monomer solution was removed, and the mixture was dried at 60°C for 10 minutes to obtain a dense polyamide Janus membrane distillation membrane, which was recorded as a dense PA / ANF Janus membrane distillation membrane.

[0086] The polytetrafluoroethylene membranes in Examples 1 and 2 and the obtained dense PA / PVA Janus membrane distillation membranes and dense PA / ANF Janus membrane distillation membranes were characterized by scanning electron microscopy. The scanning electron microscopy images of the polytetrafluoroethylene membranes are shown in Figure 1 , the SEM image of the dense PA / PVA Janus membrane distillation membrane is shown in Figure 2 , the SEM image of the dense PA / ANF Janus membrane distillation membrane is shown in Figure 3 .

[0087] Depend on Figure 1-3 It can be seen that the surface of the polytetrafluoroethylene membrane presents a porous network structure composed of nanofibers, while the surfaces of the obtained PA / PVA and PA / ANF Janus membrane distillation membranes show a dense and relatively flat structure.

[0088] Example 3

[0089] A dense polyamide Janus membrane distillation membrane (dense PA / PVAJanus membrane distillation membrane) comprises a hydrophilic modified hydrophobic membrane, a hydrophilic polyvinyl alcohol (PVA) layer and a polyamide (PA) layer arranged in sequence from bottom to top. The preparation method is the same as that in Example 1, except that step (1) is to dissolve 0.1 g of dopamine and 0.1 g of 3-aminopropyltriethoxysilane in 50 mmol / L, 50 mL of Tris-HCl buffer solution (pH=8) to obtain an activation solution, then immerse the upper surface of a polytetrafluoroethylene membrane in the activation solution, rinse the membrane surface after standing for 10 hours and dry it naturally to obtain a polytetrafluoroethylene membrane with one side hydrophilically modified. The other process steps and parameters are the same as those in Example 1.

[0090] Example 4

[0091] A dense polyamide Janus membrane distillation membrane (dense PA / ANF Janus membrane distillation membrane) comprises a hydrophilic modified hydrophobic membrane, a hydrophilic aramid nanofiber (ANF) layer and a polyamide (PA) layer arranged in sequence from bottom to top. The preparation method is the same as that of Example 2, except that step (1) comprises dissolving 0.1 g of dopamine and 0.1 g of 3-aminopropyltriethoxysilane in 50 mmol / L, 50 mL of Tris-HCl buffer solution (pH=8) to obtain an activation solution, then soaking the upper surface of a polytetrafluoroethylene membrane in the activation solution, and after standing for 10 hours, rinsing the membrane surface and drying it naturally to obtain a polytetrafluoroethylene membrane with one side hydrophilically modified. The other process steps and parameters are the same as those of Example 2.

[0092] The surface wetting properties of the compact PA / PVA and PA / ANF Janus membrane distillation membranes obtained in Examples 3 and 4 were tested. The results are as follows: Figure 4 shown.

[0093] Figure 4 The water contact angle in air and the oil contact angle underwater of the polytetrafluoroethylene membrane of Examples 3 and 4 and the dense PA / PVA and PA / ANF Janus membrane distillation membranes are shown in FIG. Figure 4 It can be seen that the polytetrafluoroethylene membrane has strong hydrophobicity, with a water contact angle of 145.7° in the air, and is oleophilic underwater, with an underwater oil contact angle of only 13.5°, which is mainly attributed to the strong hydrophobic-hydrophobic interaction between the oil droplet and the polytetrafluoroethylene membrane surface. In contrast, the surfaces of the dense PA / PVA and PA / ANF Janus membrane distillation membranes are hydrophilic in the air (water contact angles in the air are 75.8° and 69.5°), and exhibit oleophobic properties underwater (underwater oil contact angles are 136.2° and 135°), which is mainly attributed to the hydration layer formed on the surface of the dense PA / PVA and PA / ANF composite layers, which can inhibit the attachment of oil droplets, indicating that the dense PA / PVA and PA / ANF Janus membrane distillation membranes have excellent anti-oil pollution potential.

[0094] Application Example 1

[0095] The basic performance tests of the polytetrafluoroethylene membranes of Examples 3 and 4 and the dense PA / PVA and PA / ANFJanus membrane distillation membranes were carried out by direct contact membrane distillation apparatus:

[0096] The feed liquid was a 3.5 wt% sodium chloride aqueous solution, the dense PA / PVA and PA / ANF composite layers faced the feed liquid, the feed side temperature was set to 65°C, and the condensation side temperature was set to 20°C. The permeability and salt rejection of the polytetrafluoroethylene membranes of Examples 3 and 4 and the dense PA / PVA and PA / ANF Janus membrane distillation membranes were tested. The results are shown in Figure 5As shown in Figure 2, the permeation flux of the original polytetrafluoroethylene membrane is 21.0 kg·m -2 ·h -1 Since the PVA and ANF coatings exhibit hydrogel-like properties, sufficient liquid water supply is guaranteed, and the introduction of micrometer-thick coatings will not damage / sacrifice the membrane permeation flux. Therefore, when the dense ultra-thin PA layer is further introduced, the vapor flux of PA / PVA and PA / ANF Janus membrane distillation membranes (19.6 kg·m -2 ·h -1 and 19.4 kg·m -2 ·h -1 ) is only slightly lower than that of the original PTFE membrane, and the salt rejection rate is as high as 99.99%.

[0097] Example 5

[0098] A dense polyamide Janus membrane distillation membrane (dense PA / PVA Janus membrane distillation membrane) comprises a hydrophilic modified hydrophobic membrane, a hydrophilic polyvinyl alcohol (PVA) layer and a polyamide (PA) layer arranged in sequence from bottom to top. The preparation method is the same as that of Example 1, except that, in step (2), 10 g of PVA powder is added to 90 g of deionized water, and magnetic stirring is performed at 90° C. for 8 h to form a uniform PVA solution. The obtained PVA solution is poured onto one side of the hydrophilic modified polytetrafluoroethylene membrane obtained in step (1), and is evenly coated with a scraper with a gap of 50 μm, and the coating amount is 0.012 mL / cm 2 After uniform coating, the mixture was placed at 35° C. and dried for 30 minutes to obtain a hydrophilic-modified hydrophobic membrane carrying a PVA film, wherein the thickness of the PVA film was about 1 μm, and the other process steps and parameters were the same as those in Example 1.

[0099] Example 6

[0100] A dense polyamide Janus membrane distillation membrane (dense PA / ANF Janus membrane distillation membrane) comprises a hydrophilic modified hydrophobic membrane, a hydrophilic aramid nanofiber (ANF) layer and a polyamide (PA) layer arranged in sequence from bottom to top. The preparation method is the same as that of Example 2, except that in step (2), 0.4 g of KOH is completely dissolved in 0.4 mL of deionized water, and then 20 mL of dimethyl sulfoxide and 0.5 g of aramid nanofiber are added under magnetic stirring. After uniform stirring for 50 hours, a deep red ANF solution is obtained. The obtained ANF solution is poured onto one side of the hydrophilic modified polytetrafluoroethylene membrane obtained in step (1), and is evenly coated with a scraper with a gap of 50 microns, and the coating amount is 0.02 mL / cm 2The coated membrane was slowly immersed in deionized water and allowed to stand for 30 minutes, and then naturally dried to obtain a hydrophilic-modified hydrophobic membrane carrying an ANF membrane, wherein the thickness of the ANF membrane was about 1 micron, and the other process steps and parameters were the same as those in Example 2.

[0101] Application Example 2

[0102] The basic performance tests of the polytetrafluoroethylene membranes of Examples 5 and 6 and the dense PA / PVA and PA / ANFJanus membrane distillation membranes were carried out by direct contact membrane distillation apparatus:

[0103] (1) Anti-pollution performance

[0104] An aqueous solution containing 3.5 wt% sodium chloride and 1000 mg / L mineral oil was used as the feed liquid, the dense PA / PVA and PA / ANF composite layers faced the feed liquid, the feed side temperature was set to 65°C, and the condensation side temperature was set to 20°C. The anti-fouling performance of the polytetrafluoroethylene membranes of Examples 5 and 6 and the dense PA / PVA and PA / ANF Janus membrane distillation membranes was tested. The results are shown in Figure 6 and Figure 7 .

[0105] Depend on Figure 6 , Figure 7 It can be seen that due to the strong hydrophobic-hydrophobic interaction, the original PTFE membrane is easily contaminated by oil, causing its vapor flux to drop from 22.4 kg·m -2 ·h -1 The dense PA / PVA and PA / ANF Janus membranes maintained a stable steam flux (20.0 kg·m -2 ·h -1 ) and very low permeate conductivity, indicating that the two membranes have excellent anti-fouling ability. Due to the good hydration ability of the defect-free and hydrophilic PA / PVA and PA / ANF composite layers, the formed hydration layer can prevent the adhesion and infiltration of oil droplets, thereby preventing the hydrophobic substrate from contacting with oil droplets.

[0106] (2) Anti-wetting performance

[0107] A salt solution containing 3.5 wt% sodium chloride and 0.4 mM sodium dodecyl sulfate was used as the feed liquid, the dense PA / PVA and PA / ANF composite layers faced the feed liquid, the feed side temperature was set to 65°C, and the condensation side temperature was set to 20°C. The anti-wetting properties of the polytetrafluoroethylene membranes of Examples 5 and 6 and the dense PA / PVA and PA / ANF Janus membrane distillation membranes were tested. The results are shown in Figure 8 and Fig. 9 .

[0108] Depend on Figure 8 and Fig. 9 It can be seen that in the initial stage, the permeate flux and permeate conductivity of the polytetrafluoroethylene membrane increased significantly; after 30 minutes of the experiment, the permeate flux increased from 22.4 kg·m -2 ·h -1 Increased to 133.4 kg·m -2 ·h -1 , the conductivity of the permeate increased from 3.2μS / cm to 5895.5μS / cm, indicating that the polytetrafluoroethylene membrane was severely wetted and the feed liquid directly passed through the hydrophobic membrane into the permeate side in liquid form. In contrast, the dense PA / PVA and PA / ANF Janus membrane distillation membranes have excellent anti-wetting properties. After 24 hours of the experiment, the permeate side still maintained a very low conductivity of 25.2μS / cm and 2.2μS / cm, respectively.

[0109] Example 7

[0110] A dense polyamide Janus membrane distillation membrane (dense PA / PVA Janus membrane distillation membrane) comprises a hydrophilic modified hydrophobic membrane, a hydrophilic polyvinyl alcohol (PVA) layer and a polyamide (PA) layer arranged in sequence from bottom to top. The preparation method is the same as that of Example 3, except that, in step (3), piperazine is dissolved in deionized water and mixed by ultrasound to obtain an aqueous phase monomer solution, wherein the concentration of piperazine in the aqueous phase monomer solution is 1wt%; trimesoyl chloride is dissolved in n-hexane and mixed by ultrasound to obtain an oil phase monomer solution, wherein the concentration of trimesoyl chloride in the oil phase monomer solution is 0.1wt%. Other process steps and parameters are the same as those of Example 3.

[0111] Example 8

[0112] A dense polyamide Janus membrane distillation membrane (dense PA / ANF Janus membrane distillation membrane) comprises a hydrophilic modified hydrophobic membrane, a hydrophilic aramid nanofiber (ANF) layer and a polyamide (PA) layer arranged in sequence from bottom to top. The preparation method is the same as that of Example 4, except that, in step (3), piperazine is dissolved in deionized water and mixed by ultrasound to obtain an aqueous monomer solution, wherein the concentration of piperazine in the aqueous monomer solution is 1wt%; trimesoyl chloride is dissolved in n-hexane and mixed by ultrasound to obtain an oily monomer solution, wherein the concentration of trimesoyl chloride in the oily monomer solution is 0.1wt%. The other process steps and parameters are the same as those of Example 4.

[0113] Application Example 3

[0114] The basic performance tests of the polytetrafluoroethylene membranes of Examples 7 and 8 and the dense PA / PVA and PA / ANFJanus membrane distillation membranes were carried out by direct contact membrane distillation apparatus:

[0115] A salt solution containing 3.5 wt% sodium chloride, 1000 mg / L mineral oil and 0.4 mM sodium dodecyl sulfate (SDS) was used as the feed liquid. The dense PA / PVA and PA / ANF composite layers faced the feed liquid. The feed side temperature was set to 65°C and the condensation side temperature was set to 20°C. The anti-fouling and anti-wetting properties of the polytetrafluoroethylene membranes of Examples 7 and 8 and the dense PA / PVA and PA / ANF Janus membrane distillation membranes were tested. The results are shown in Table 1. Fig.10 , Fig.11 .

[0116] Depend on Fig.10 , Fig.11 It can be seen that for the PTFE membrane, the steam flux increased fourfold within the initial 15 min, indicating that SDS caused severe membrane pore wetting. Due to the increased oil contamination, the steam flux decreased significantly and the conductivity increased significantly to 6468.0 μS / cm. Compared with the original PTFE membrane, the dense PA / PVA and PA / ANF Janus membrane distillation membranes have better ability to resist both contamination and wetting. In the 100-h membrane distillation test, the flux of the PA / PVA Janus membrane distillation membrane slowly decreased (reduced by 10.3 kg·m -2 ·h -1 ), the conductivity of the distillate increased slightly. The PA / ANF Janus membrane distillation membrane has a more stable evaporation flux (~20.5kg·m -2 ·h -1 ) and lower effluent conductivity. Thanks to the high capillary pressure and hydration capacity of the dense and complete PA / ANF composite layer, the direct contact between SDS and oil and the hydrophobic substrate can be prevented by inhibiting the diffusion of surfactants and intercepting oil pollution by the hydration layer, thus achieving long-term, robust and efficient membrane distillation treatment of high-salinity emulsions containing surfactant-stabilized oil.

[0117] Comparative Example 1

[0118] A polyamide Janus membrane distillation membrane comprises a hydrophilic-modified hydrophobic membrane and a polyamide (PA) layer arranged in sequence from bottom to top, and a preparation method comprises the following steps:

[0119] (1) 0.1 g dopamine and 0.1 g polyethyleneimine were dissolved in 50 mmol / L, 50 mL Tris-HCl buffer solution (pH=8) to obtain an activation solution, and then the upper surface of the polytetrafluoroethylene membrane was immersed in the activation solution. After standing for 12 hours, the membrane surface was rinsed and naturally dried to obtain a polytetrafluoroethylene membrane with one side hydrophilically modified;

[0120] (2) dissolving m-phenylenediamine in deionized water and stirring to mix the solution to obtain an aqueous monomer solution, wherein the concentration of m-phenylenediamine in the aqueous monomer solution is 2 wt %, dissolving trimesoyl chloride in n-hexane and mixing the solution by ultrasonication to obtain an oily monomer solution, wherein the concentration of trimesoyl chloride in the oily monomer solution is 0.2 wt %;

[0121] (3) The hydrophilically modified polytetrafluoroethylene membrane prepared in step (1) is fixed on a polytetrafluoroethylene membrane, and then the aqueous monomer solution prepared in step (2) is uniformly dripped onto one side of the hydrophilically modified polytetrafluoroethylene membrane. After standing for 5 minutes, the excess aqueous monomer solution is removed and the membrane is naturally dried. Then, the oily monomer solution prepared in step (3) is continuously dripped onto the surface of the membrane, spread evenly, and then stood for 2 minutes. The excess oily monomer solution is removed and the membrane is dried at 60° C. for 10 minutes to obtain a polyamide Janus membrane distillation membrane, referred to as a PAJanus membrane distillation membrane.

[0122] Application Example 4

[0123] The liquid entry pressure value test was performed on the dense PA / PVA Janus membrane distillation membrane and polytetrafluoroethylene membrane of Example 1, the PA / ANF Janus membrane distillation membrane of Example 2, and the PA Janus membrane distillation membrane of Comparative Example 1 by using a pressure testing device. The results are shown in Fig.12 .

[0124] Liquid ingress pressure test is often used to evaluate the important parameters of membrane distillation membrane anti-wetting performance. Fig.12 It can be found that the liquid entry pressure value of the polytetrafluoroethylene membrane is 2.9±0.2 bar, while the liquid entry pressure value of the PAJanus membrane distillation membrane of comparative example 1 increases to 4.3±0.1 bar. In contrast, the liquid entry pressure of the compact PA / PVA and PA / ANF Janus membrane distillation membranes of Examples 1 and 2 increases significantly to 9.0±0.2 bar and 9.8±0.5 bar, respectively. This is mainly attributed to the double-layer barrier effect and capillary effect of the hydrophilic middle layer and the compact polyamide layer.

[0125] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A dense polyamide Janus membrane distillation membrane, characterized in that: The invention comprises a hydrophilic modified hydrophobic film, a hydrophilic middle layer and a polyamide layer which are arranged in sequence from bottom to top, wherein the hydrophilic middle layer is a polyvinyl alcohol layer or an aramid nanofiber layer.

2. The dense polyamide Janus membrane distillation membrane according to claim 1, characterized in that The hydrophilic-modified hydrophobic membrane comprises one of a hydrophilic-modified polytetrafluoroethylene membrane, a polyvinylidene fluoride membrane, a polypropylene membrane and a composite membrane thereof.

3. A method for preparing a dense polyamide Janus membrane distillation membrane according to any one of claims 1 to 2, characterized in that: The hydrophilic intermediate layer solution is uniformly coated on the surface of one side of the hydrophobic membrane that has been hydrophilically modified to obtain a hydrophilic intermediate layer, and then the aqueous phase monomer solution and the oil phase monomer solution are sequentially infiltrated into the surface of the hydrophilic intermediate layer by interfacial polymerization reaction to form a polyamide layer, thereby obtaining the dense polyamide Janus membrane distillation membrane; The hydrophilic intermediate layer solution is a polyvinyl alcohol solution or an aramid nanofiber solution.

4. The method for preparing a dense polyamide Janus membrane distillation membrane according to claim 3, characterized in that: The polyvinyl alcohol solution is obtained by uniformly mixing polyvinyl alcohol and deionized water; The aramid nanofiber solution is obtained by dissolving potassium hydroxide in deionized water and then adding dimethyl sulfoxide and aramid nanofiber under magnetic stirring.

5. The method for preparing a dense polyamide Janus membrane distillation membrane according to claim 4, characterized in that: The mass concentration of the polyvinyl alcohol solution is 6-12%, the usage ratio of potassium hydroxide to deionized water is 0.5-2 g / mL, the mass ratio of potassium hydroxide to aramid nanofiber is (0.5-2):1, and the usage ratio of aramid nanofiber to dimethyl sulfoxide is 0.01-0.04 g / mL.

6. The method for preparing a dense polyamide Janus membrane distillation membrane according to claim 3, characterized in that: The aqueous monomer solution is a polyamine aqueous solution with a mass concentration of 0.5-2%, and the polyamine is one of piperazine, m-phenylenediamine or polyethyleneimine.

7. The method for preparing a dense polyamide Janus membrane distillation membrane according to claim 3, characterized in that: The oil phase monomer solution is a mixed solution of a polyacyl chloride and an organic solvent, wherein the mass concentration of the polyacyl chloride in the oil phase monomer solution is 0.02-0.3%, the polyacyl chloride is one of trimesoyl chloride, isophthaloyl chloride, cyclohexanetrichloride, cyclopentanetrichloride, propanetrichloride or glutaryltrichloride, and the organic solvent is one of n-hexane, n-heptane, dodecane or tetradecane.

8. The method for preparing a dense polyamide Janus membrane distillation membrane according to claim 3, characterized in that: The coating amount of the hydrophilic intermediate layer solution is 0.01-0.02 mL / cm 2 The amount of the aqueous monomer solution used during infiltration is 0.15-0.25 mL / cm 2 The amount of the oil phase monomer solution used during infiltration is 0.15-0.25 mL / cm 2 .

9. The method for preparing a dense polyamide Janus membrane distillation membrane according to claim 3, characterized in that: The following steps are involved: The hydrophilic intermediate layer solution is uniformly coated on one surface of the hydrophilic modified hydrophobic membrane, and after drying, a hydrophilic modified hydrophobic membrane carrying the hydrophilic intermediate layer is obtained; The hydrophilic modified hydrophobic membrane carrying the hydrophilic intermediate layer is fixed, then uniformly infiltrated with an aqueous monomer solution, allowed to stand and then dried, and then continued to be uniformly infiltrated with a uniform oil phase monomer solution, allowed to stand and then dried to obtain the dense polyamide Janus membrane distillation membrane.

10. Use of the dense polyamide Janus membrane distillation membrane according to any one of claims 1 to 2 in membrane distillation.

Citation Information

Patent Citations

  • Thin-layer composite membrane for anti-wetting membrane distillation as well as preparation method and application of thin-layer composite membrane

    CN116020267A

  • Preparation method of anti-pollution and wetting-resistant composite distillation membrane

    CN116036887A

  • Alg / M hydrogel composite membrane as well as preparation method and application thereof

    CN116832625A

  • Asymmetric composite membranes and modified substrates used in their preparation

    WO2019186518A1