Chitosan modified porous material as well as preparation method and application thereof
By combining chitosan with porous support matrix and silicone rubber, a three-dimensional network structure chitosan modified porous material was prepared, which solved the problem of single adsorption objects and limited effects in the prior art, and achieved heavy metals, dyes and Continuous adsorption of proteins improves wastewater treatment efficiency and reduces costs.
Patent Information
- Application Number
- CN202410957646.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-01
AI Technical Summary
Existing chitosan adsorbent materials can only adsorb one or a type of pollutants, and the adsorption effect is limited, and the continuous treatment of sewage cannot be achieved, limiting its application in sewage treatment.
By combining chitosan and/or its derivatives with a porous support matrix and silicone rubber, a chitosan modified porous material with a three-dimensional network structure is prepared, which continuously adsorbs heavy metals, dyes and proteins in wastewater.
It has achieved excellent adsorption effect on many types of pollutants, and can continuously treat sewage without producing sludge and concentrated wastewater, significantly improve treatment efficiency, and has low preparation cost, simple process, and meets environmental protection requirements.
Smart Images

Figure CN118874433A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sewage treatment materials, and in particular relates to a chitosan modified porous material and a preparation method and application thereof. Background Art
[0002] As the scope and frequency of human production activities expand, the content of pollutants in water bodies increases, which continuously threatens the biosphere of the entire earth, causing huge economic losses and being the direct cause of many diseases and deaths. Heavy metals are the most harmful pollutants that exist in large quantities in many water systems, which can cause water quality to deteriorate or deteriorate. Heavy metals are easily absorbed and enriched by organisms and can be amplified step by step through the food chain. In addition to heavy metal pollutants, emissions from human activities such as proteins and dyes can also directly or indirectly pollute precious water resources.
[0003] Traditional sewage treatment methods include chemical precipitation, coagulation sedimentation, adsorption, electrodialysis, flotation, etc., which have the problems of needing to collect sewage in advance, high cost and difficulty in separation, or requiring more complicated process methods and harsh implementation conditions, and cannot form a universal method for controlling water pollution.
[0004] Chitosan is a natural macromolecular polysaccharide with a wide range of sources. As a polysaccharide second only to cellulose in nature, it is mainly extracted from crustaceans, which makes it have a lower production cost. In addition, by modifying chitosan, water-soluble derivatives such as carboxymethyl chitosan, hydroxypropyl chitosan, and chitosan lactate are obtained, further expanding its scope of application. Chitosan itself has good biodegradability, which is also in line with the contemporary pursuit of sustainability and environmental protection. As a flocculant, chitosan has the advantages of fast flocculation speed, low flocculation temperature, strong adsorption capacity, and large surface area. It is expected to be used for efficient removal of impurities and suspended matter in water to improve water quality. CN 102671633 A discloses a chitosan aluminum-iron composite adsorbent prepared by cross-linking chitosan combined with iron and aluminum salts with glutaraldehyde, which can be used to remove fluoride ions in fluoride-containing wastewater. CN 109794226A discloses a hydrothermal carbonized chitosan sphere adsorbent, which has an excellent adsorption effect on heavy metal Cr ions and can be maintained in an acidic aqueous solution for more than 10 days.
[0005] However, the chitosan adsorption materials mentioned above can only adsorb one or one type of pollutants, the adsorption object is single, the adsorption effect is limited, and continuous sewage treatment cannot be performed, which greatly limits the application of chitosan materials in sewage treatment. Therefore, a chitosan adsorption material with good adsorption effect and capable of continuous sewage treatment is still to be developed. Summary of the invention
[0006] The purpose of the present invention is to provide a chitosan modified porous material and a preparation method and application thereof in order to overcome the defects of the prior art in that the adsorption object is single and the adsorption effect is limited.
[0007] The purpose of the present invention can be achieved by the following technical solutions:
[0008] The invention provides a chitosan modified porous material, comprising a porous supporting matrix having a three-dimensional network structure on which chitosan and / or chitosan derivatives and silicone rubber are loaded.
[0009] Furthermore, the porous material has a pore size of 50-200 μm and a porosity of 90-95%.
[0010] Furthermore, the porous support matrix includes one or more of polyurethane sponge, amino polyacrylonitrile sponge, chitosan sponge or melamine sponge, preferably polyurethane sponge.
[0011] Furthermore, the chitosan derivative includes one or more of carboxymethyl chitosan, chitosan hydrochloride, quaternary ammonium salt chitosan or hydroxypropyl chitosan, preferably carboxymethyl chitosan.
[0012] Furthermore, the molecular weight of the chitosan and / or chitosan derivative is 100-600 kDa.
[0013] The present invention also provides a method for preparing a chitosan-modified porous material, comprising the following steps:
[0014] S1: dissolving chitosan and / or chitosan derivatives in water, and then adding silicone rubber and mixing evenly;
[0015] S2: adding a curing agent to the mixed solution of S1, and mixing to obtain a prepolymer solution;
[0016] S3: fully immersing the dried porous support substrate in the prepolymer solution of S2, taking it out and solidifying it to obtain the chitosan modified porous material.
[0017] Furthermore, in step S1, the mass ratio of chitosan and / or chitosan derivative to water is 1:(3-5).
[0018] Furthermore, in step S1, the mass ratio of chitosan and / or chitosan derivative to silicone rubber is 1:(5-80), preferably 1:(10-30).
[0019] Furthermore, in step S2, the added amount of the curing agent is 3%-5% of the mass of the silicone rubber.
[0020] Furthermore, in step S3, the porous support matrix is dried at 100-110° C. for 1-2 hours.
[0021] Furthermore, in step S3, the specific process of curing is: first curing at room temperature for 10-20 minutes, and then curing at 80-90° C. for 2-3 hours.
[0022] Furthermore, in step S3, during curing at 80-90° C., the film is turned over every 20-30 minutes to ensure uniform curing.
[0023] Furthermore, the curing agent used in the curing is vinyltributylidene oxime silane, which is used to cure the silica gel to obtain a chitosan-modified porous material with good mechanical properties.
[0024] The present invention also provides an application of a chitosan modified porous material in sewage treatment. The chitosan modified porous material can be used to absorb heavy metals, dyes and proteins in sewage.
[0025] Furthermore, the application process of the chitosan modified porous material is specifically as follows:
[0026] like Figure 1 As shown, the chitosan modified porous material is connected to the water inlet pipe of the pump and placed in the sewage containing pollutants, and the water outlet pipe of the pump is also placed in the sewage containing pollutants. After the power is turned on, the sewage containing pollutants circulates continuously inside the chitosan modified porous material, and the chitosan and / or chitosan derivatives modified on the three-dimensional network structure inside the porous material can continuously adsorb pollutants in the sewage.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] (1) The present invention uses chitosan and / or chitosan derivatives to modify the porous material matrix, and the prepared porous material can be used to adsorb various pollutants such as metal ions, dyes and proteins in sewage, and has excellent adsorption effect.
[0029] (2) The present invention uses chitosan and / or chitosan derivatives for modification. The hydroxyl and amino functional groups in the chitosan molecular structure provide the ability to bind to heavy metal ions, and chitosan can form hydrogen bonds with protein molecules for adsorption. The adsorption performance and application range of chitosan derivatives can be further enhanced.
[0030] (3) The present invention also adds silicone rubber during the preparation process of the modified porous material. Silicone rubber can resist various substances such as acid, alkali, solvent, chemicals and water, and is an inert material with excellent performance. Adding silicone rubber to the modified porous material can extend the service life of the material and provide a bonding effect for the modified load of chitosan. The silicone rubber is converted from liquid to solid under the action of the curing agent, and the chitosan and / or chitosan derivatives are fixed inside the sponge.
[0031] (4) The chitosan-modified porous material prepared in the present invention can allow pollutants to enter the adsorption site well during sewage treatment and evenly adhere to the internal pores, and can effectively adsorb various pollutants from water without generating sludge and concentrated wastewater.
[0032] (5) The chitosan-modified porous material of the present invention still has good mechanical properties after completing the adsorption of pollutants, can realize the continuous treatment of sewage, significantly improve the treatment efficiency, and has low preparation cost, simple process, green and pollution-free preparation process, and broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a schematic diagram of the application process of the chitosan modified porous material of the present invention for pollutant adsorption.
[0034] Figure 2 These are optical microscope photos of the chitosan-modified porous material of Example 2 of the present invention before and after modification.
[0035] Figure 3 This is a test chart of the adsorption performance of the porous materials of Examples 1-2 of the present invention and Comparative Example 1 on different pollutants.
[0036] Figure 4 This is a graph showing the absorbance of sewage before and after the modified porous material of Example 2 of the present invention adsorbs pollutants.
[0037] Figure 5 This is a before and after comparison diagram of the modified porous material of Example 2 of the present invention adsorbing different pollutants.
[0038] Figure 6 These are stress-strain curves of the porous materials of Examples 1-2 and Comparative Example 1 of the present invention.
[0039] Figure 7 1 is the stress-strain curve of the modified porous material of Example 2 of the present invention after adsorbing different pollutants. DETAILED DESCRIPTION
[0040] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0041] Unless otherwise specified, the reagents, methods, instruments and equipment used in the present invention are conventional reagents, methods, instruments and equipment in the art. Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0042] Embodiment 1:
[0043] This embodiment provides a chitosan modified porous material, and the specific preparation method is as follows:
[0044] S1: Use a cylindrical die cutter to cut the polyurethane sponge substrate into suitable sizes, place it in an electric hot air drying oven, set the temperature to 100°C and dry it for 1.5 hours.
[0045] S2: Weigh a certain amount of chitosan (molecular weight 150 kDa) and add 3 times the amount of water to fully swell it to obtain a chitosan solution with a concentration of 25 wt%. Then slowly add silicone rubber to the chitosan solution and mix well to obtain a chitosan / silicone rubber mixed solution. The mass ratio of chitosan to silicone rubber is 1:10.
[0046] S3: Add curing agent (vinyl trisbutyl ketoxime silane) to the chitosan / silicone rubber mixture, stir thoroughly for 2 minutes to obtain chitosan / silicone rubber prepolymer solution, wherein the amount of curing agent added is 4% of the mass of the silicone rubber in the mixture.
[0047] S4: Take out the completely dried polyurethane sponge matrix, place it in the chitosan / silicone rubber prepolymer liquid, squeeze it repeatedly to fully absorb it, and after saturation, cure it at room temperature for 10 minutes, and then put it in an oven set at 80°C to cure for 3 hours. During this period, turn it over every 20 minutes to ensure uniform curing. The finished product is obtained after complete curing.
[0048] Embodiment 2:
[0049] This embodiment provides a porous material modified with carboxymethyl chitosan, and the specific preparation method is as follows:
[0050] S1: Use a cylindrical die cutter to cut the polyurethane sponge substrate into suitable sizes, place it in an electric hot air drying oven, set the temperature to 100°C and dry it for 1.5 hours.
[0051] S2: Weigh a certain amount of carboxymethyl chitosan (molecular weight 500 kDa) and add 3 times the amount of water to fully swell it to obtain a carboxymethyl chitosan solution with a concentration of 25wt%. Then slowly add silicone rubber to the carboxymethyl chitosan solution and mix well to obtain a carboxymethyl chitosan / silicone rubber mixed solution. The mass ratio of carboxymethyl chitosan to silicone rubber is 1:30.
[0052] S3: Add curing agent (vinyl trisbutyl ketoxime silane) to the carboxymethyl chitosan / silicone rubber mixture, and stir for 2 minutes to obtain a carboxymethyl chitosan / silicone rubber prepolymer solution, wherein the amount of curing agent added is 5% of the mass of the silicone rubber in the mixture.
[0053] S4: Take out the completely dried polyurethane sponge matrix, place it in carboxymethyl chitosan / silicone rubber prepolymer liquid, squeeze it repeatedly to fully absorb it, and after saturation, cure it at room temperature for 10 minutes, and then put it in an oven set at 80°C to cure for 3 hours. During this period, turn it over every 20 minutes to ensure uniform curing. The finished product is obtained after complete curing.
[0054] The optical microscope schematic diagram of the porous material modified with carboxymethyl chitosan prepared in this example is shown in Figure 2 The left picture shows the unmodified sponge, which has a dry and smooth surface and a distinct outline. After the sponge is modified, the microscopic morphology of the sponge is as follows: Figure 2 As shown in the right picture, it can be seen that a layer of transparent carboxymethyl chitosan mixture is evenly attached to the inside, the surface becomes moist, and the pores are unobstructed, which allows pollutants to enter the adsorption sites well and adhere evenly between the internal pores. It can effectively adsorb various pollutants from the water without generating sludge and concentrated wastewater.
[0055] Embodiment 3:
[0056] This embodiment provides a porous material modified with carboxymethyl chitosan. The preparation method is basically the same as that of Example 2, except that the mass of water added in step S2 of this embodiment is 5 times that of carboxymethyl chitosan.
[0057] Embodiment 4:
[0058] This embodiment provides a porous material modified by carboxymethyl chitosan. The preparation method is basically the same as that of Embodiment 2, except that the mass ratio of carboxymethyl chitosan to silicone rubber in step S2 of this embodiment is 1:50.
[0059] Embodiment 5:
[0060] This embodiment provides a porous material modified by carboxymethyl chitosan. The preparation method is basically the same as that of Embodiment 2, except that the mass ratio of carboxymethyl chitosan to silicone rubber in step S2 of this embodiment is 1:80.
[0061] Comparative Example 1:
[0062] The porous material in this comparative example is not modified with chitosan, that is, a pure polyurethane sponge matrix.
[0063] Comparative Example 2:
[0064] This comparative example provides a carboxymethyl chitosan modified porous material, and the specific preparation method is as follows:
[0065] S1: Use a cylindrical die cutter to cut the polyurethane sponge substrate into suitable sizes, place it in an electric hot air drying oven, set the temperature to 100°C and dry it for 1.5 hours.
[0066] S2: Weigh a certain mass of carboxymethyl chitosan and add 3 times the mass of water to fully swell it, to obtain a carboxymethyl chitosan solution with a concentration of 25 wt%.
[0067] S3: Take out the completely dried polyurethane sponge matrix, place it in the carboxymethyl chitosan solution and squeeze it repeatedly to fully absorb it.
[0068] However, it was found during the preparation process that the carboxymethyl chitosan solution absorbed by the polyurethane sponge matrix without silicone rubber was only 60% of that when silicone rubber was added, and when the polyurethane sponge was immersed in sewage for a long time to absorb pollutants, the carboxymethyl chitosan attached to the porous material would fall into the sewage after swelling, thus rendering the porous material ineffective. Therefore, silicone rubber must be added to effectively fix chitosan and / or chitosan derivatives inside the sponge.
[0069] The present invention performs the following adsorption tests on Examples 1-2 and Comparative Example 1:
[0070] (1) Heavy metal adsorption test: Taking copper ion as an example, take 150mL of copper sulfate solution (10mg mL -1 ), through a homemade circulating filtration device ( Figure 1 ), the use volume is 9cm 3 The modified porous material was adsorbed for 20 minutes. Using JASCO V750 UV-visible spectrophotometer, the temperature was fixed at 25°C, the wavelength range was 200-400nm, and the absorbance of the solution was recorded. The adsorption rate was calculated as follows:
[0071]
[0072] (2) Dye adsorption test: Taking methyl orange as an example, take 150 mL of methyl orange solution (6 mg mL -1 ), the use volume is 9cm 3 The modified porous material was adsorbed for 20 minutes, and the absorbance of the solution was recorded after full spectrum testing. The adsorption rate of methyl orange was calculated according to the formula in (1).
[0073] (3) Protein adsorption: Taking bovine serum albumin (BSA) as an example, 150 mL of bovine serum albumin solution (BSA, 2 mg mL -1 ), the use volume is 9cm 3 The modified porous material was adsorbed for 20 minutes, and after a full spectrum test to record the absorbance of the solution, the adsorption rate of BSA was obtained by calculation.
[0074] The present invention also conducts mechanical property tests on the porous materials prepared in Example 2 and the comparative example after adsorbing different pollutants. The specific test process is as follows: a compression test is conducted on the sponge after adsorption using a TA Q800 electronic universal testing machine. After selecting the sample shape as a cylinder in the instrument supporting software, input its radius and thickness, and set the compression rate to 5 mm·s -1 , after compressing the sponge, its stress-strain curve is obtained.
[0075] The adsorption effects of the porous materials of Examples 1-2 and Comparative Example 1 are as follows: Figure 3-5 As shown in Figure 2, for the adsorption of heavy metals, taking copper ions as an example, the adsorption rate of pure polyurethane sponge (Comparative Example 1) is only 0.23 mg·cm -3 ·min -1 After modification with chitosan (Example 1), the adsorption rate increased to 2.81 mg cm -3 ·min -1 After modification with carboxymethyl chitosan (Example 2), the adsorption rate further increased to 6.42 mg cm -3 ·min -1 For dye adsorption, taking methyl orange as an example, the adsorption rates are 0.14 mg·cm -3 ·min -1 , 1.27 mg cm -3 ·min -1 and 3.58 mg cm -3 ·min -1 For protein adsorption, taking bovine serum albumin as an example, the adsorption capacity is 0.03 mg·cm -3 ·min -1 , 0.46 mg cm -3 ·min -1 and 1.28 mg cm -3 ·min -1. It can be found that if the polyurethane sponge is not modified with chitosan and / or chitosan derivatives, the polyurethane sponge itself has little adsorption effect on pollutants. After modification with chitosan, for heavy metal ions, since the surface of chitosan molecules carries positive charges, they can interact with the negative charges of heavy metal ions to form an adsorption layer on the surface to achieve adsorption; and chitosan molecules have rich functional groups, such as amino and hydroxyl groups, which can form coordination bonds with heavy metals to achieve adsorption of heavy metals; for dyes, the porous structure of chitosan also provides a large number of adsorption sites for dye molecules, so that dye molecules can be effectively adsorbed on its surface or filtered out; for proteins, chitosan can form hydrogen bonds with protein molecules for adsorption. Modification with chitosan derivatives can further enhance its adsorption performance.
[0076] The mechanical properties of the porous materials of Examples 1-2 and Comparative Example 1 are as follows Figure 6-7 As shown. When compressed to 90% of the original sample, the compressive stress of the pure polyurethane sponge (Comparative Example 1) is only 0.06MPa. After modification with chitosan (Example 1), its compressive stress rises to 1.31MPa. After modification with carboxymethyl chitosan (Example 2), it further rises to 1.72MPa. It can be found that if the polyurethane sponge is not modified with chitosan and / or chitosan derivatives, the mechanical properties of the polyurethane sponge are poor and cannot withstand the force applied to the porous material during pumping during actual sewage treatment. After modification with chitosan and / or chitosan derivatives, its mechanical properties are improved by 21-28 times, meeting the mechanical property requirements of sewage treatment in conventional occasions. The compressive stresses at 90% compressive strain after absorbing methyl orange and bovine serum albumin are 1.73MPa and 2.01MPa respectively, and the mechanical properties are slightly improved; the compressive stress at 90% compressive strain after absorbing copper ions is 4.65MPa, which is due to the formation of coordination bonds between copper ions and amino and hydroxyl groups in chitosan molecules, which greatly improves the mechanical properties of porous materials.
[0077] In summary, the present invention uses chitosan and its derivatives to modify polyurethane sponge, and prepares a three-dimensional porous material that can be used to adsorb heavy metal ions, dyes and proteins. It can effectively adsorb various pollutants from water without generating sludge and concentrated wastewater. The modified porous material prepared by the present invention still has a porosity of 90-95% to meet the continuous and efficient circulation of sewage inside the material, thereby effectively adsorbing heavy metal ions, dyes and proteins in sewage. The adsorption effect is different for different substances. By comparing the swelling degree before and after adsorption, it can be concluded that the modified three-dimensional porous material has a good adsorption effect on copper sulfate, methyl orange and bovine serum albumin. The mechanical properties of the modified porous material are good, and its mechanical properties are further improved after adsorbing pollutants, which fully meets the mechanical performance requirements of sewage treatment in conventional occasions, and has broad application prospects in the field of sewage treatment.
[0078] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A chitosan modified porous material, characterized in that: The invention comprises a porous support matrix having a three-dimensional network structure, and the three-dimensional network structure is loaded with chitosan and / or chitosan derivatives and silicone rubber.
2. The chitosan modified porous material according to claim 1, characterized in that: The porous support matrix includes one or more of polyurethane sponge, amino polyacrylonitrile sponge, chitosan sponge or melamine sponge.
3. The chitosan modified porous material according to claim 1, characterized in that: The chitosan derivatives include one or more of carboxymethyl chitosan, chitosan hydrochloride, quaternary ammonium salt chitosan or hydroxypropyl chitosan.
4. A method for preparing a chitosan-modified porous material according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1: dissolving chitosan and / or chitosan derivatives in water, and then adding silicone rubber and mixing evenly; S2: adding a curing agent to the mixed solution of S1, and mixing to obtain a prepolymer solution; S3: Immersing the dried porous support substrate in the prepolymer solution of S2, taking it out and solidifying it to obtain the chitosan modified porous material.
5. The method for preparing a chitosan modified porous material according to claim 3, characterized in that: In step S1, the mass ratio of chitosan and / or chitosan derivative to water is 1:(3-5).
6. The method for preparing a chitosan-modified porous material according to claim 3, characterized in that: In step S1, the mass ratio of chitosan and / or chitosan derivative to silicone rubber is 1:(5-80).
7. The method for preparing a chitosan-modified porous material according to claim 3, characterized in that: In step S2, the added amount of the curing agent is 3%-5% of the mass of the silicone rubber.
8. The method for preparing a chitosan-modified porous material according to claim 3, characterized in that: In step S3, the porous support substrate is dried at 100-110° C. for 1-2 hours.
9. The method for preparing a chitosan-modified porous material according to claim 3, characterized in that: In step S3, the specific process of curing is: first curing at room temperature for 10-20 minutes, and then curing at 80-90°C for 2-3 hours.
10. An application of the chitosan modified porous material according to any one of claims 1 to 3 in sewage treatment, characterized in that: The porous material is used for adsorbing heavy metals, dyes and proteins in sewage.
Citation Information
Patent Citations
Preparation method, product and application of chitosan aluminum-iron composite adsorbent
CN102671633A
Hydrothermal charred chitosan sphere adsorbent and preparation method and application thereof
CN109794226A
Method for preparing polyurethane / chitosan composite foam and application of polyurethane / chitosan composite foam
CN102921394A
Modified rice hull ash-silicone rubber composite material and preparation method thereof
CN105400199A
Porous superhydrophobic oil-absorption magnetic separation material and preparation method thereof