Preparation method of flexible reticular water treatment material

By coating the gallium-tungsten-cerium ternary composite oxide active coating on the alumina fiber mesh, a flexible mesh water treatment material was prepared, which solved the problem that the mesh material could not be regenerated after adsorption and saturation in the prior art. It achieves the effect of efficient decomposition of organic pollutants under light and is suitable for continuous purification of wastewater.

CN118874444APending Publication Date: 2024-11-01SHENYANG LIGONG UNIV

Patent Information

Application Number
CN202410934621.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing mesh materials cannot continue to play a purification role after being saturated with adsorbed organic pollutants, and the regeneration process is complicated and is not suitable for large-scale continuous treatment of wastewater.

Method used

A flexible mesh water treatment material is prepared by coating the active coating of gallium-tungsten-cerium ternary oxide, which can decompose organic pollutants under light. It is suitable for Continuous purification of wastewater.

Benefits of technology

This material has the ability to efficiently decompose organic pollutants on the basis of retaining the strength and corrosion resistance of the alumina fiber web. It is suitable for the removal and purification of a variety of organic pollutants, and its structure and performance are stable below 550°C.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a preparation method of a flexible reticular water treatment material, and belongs to the field of environmental pollution purification materials. The method comprises the following process steps: activating an alumina fiber net, preparing a gallium-tungsten-cerium precursor, and laminating the fiber net. By optimizing the raw materials and the preparation process, the gallium-tungsten-cerium ternary composite oxide active coating with photocatalytic purification activity is prepared on the activated alumina fiber mesh, and the coating is high in binding force with the activated alumina fiber mesh and good in compatibility. The prepared flexible net-shaped water treatment material has the capability of decomposing and purifying organic pollutants in water under illumination on the basis of keeping the strength, corrosion resistance and flexibility of the alumina fiber net. The flexible net-shaped water treatment material can be widely used for removing and purifying various organic pollutants in water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of environmental pollution purification materials, and in particular relates to a method for preparing a flexible mesh water treatment material. Background Art

[0002] Organic pollutants in water mainly come from industrial and domestic sewage. Toxic and harmful organic pollutants pose a huge threat to human health. Effective measures must be taken to purify them before they are discharged into environmental water bodies.

[0003] Mesh materials play an important role in water pollution control. This material can be fixed in a water treatment device and can remove organic pollutants from the water when water flows through it. Mesh materials mainly remove organic pollutants from water by adsorption, and the strength of the adsorption capacity depends on the composition and structure of the mesh material. The main problem with the adsorption purification method is that the mesh material can no longer play a purification role after it is saturated with organic matter. The commonly used method is to regenerate the mesh material, such as heating or eluting with a solvent. However, both of these regeneration methods require the mesh material to be removed from the wastewater, which increases the complexity of the operation and is not suitable for large-scale continuous wastewater treatment. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention aims to provide a method for preparing a flexible mesh water treatment material, which can be used for purifying and treating organic pollutants in water.

[0005] A method for preparing a flexible mesh water treatment material comprises the following process steps:

[0006] Step 1: Activation of Alumina Fiber Mesh

[0007] The treated alumina fiber mesh was dried at 150° C. for 10 h, and then calcined at 580-600° C. for 2 h to obtain an activated alumina fiber mesh;

[0008] Step 2: Prepare Gallium-Tungsten-Cerium Precursor

[0009] (1) Add 105-135 mL of ethanol, 5.5-6.3 mL of isopropanol, and 3.2-3.8 g of polyethylene glycol with a molecular weight of 10,000 to a beaker in sequence and stir to form solution B;

[0010] (2) Add 235-245 mL of pure water, 7.2-8.3 g of gallium nitrate, 5.7-6.2 g of sodium tungstate, and 4.3-4.6 g of cerium nitrate hexahydrate into a beaker and stir to form a solution C;

[0011] (3) Add 3.5-3.9 g of octadecyltrimethylammonium chloride to solution C and stir to form solution D;

[0012] (4) mixing solution B and solution D, placing in a constant temperature water bath at 85° C. and stirring for 30 min to prepare a gallium-tungsten-cerium precursor;

[0013] Step 3: Fiber Mesh Lamination

[0014] (1) immersing the activated alumina fiber mesh obtained in step 1 into a gallium-tungsten-cerium precursor, keeping it in a constant temperature water bath at 85° C. for 30 min, and then taking it out and washing it with pure water;

[0015] (2) The cleaned fiber web is dried at 150° C. for 10 h, and then calcined at 550-570° C. for 2 h to obtain a flexible mesh water treatment material.

[0016] Furthermore, the alumina fiber mesh described in step 1 is a grid-shaped mesh woven from alumina fibers with a diameter of 1 mm, with a spacing of 1.5 mm between the alumina fibers, and can withstand a high temperature of 1000°C.

[0017] Furthermore, the alumina fiber mesh processing process described in step 1 is:

[0018] (1) Add 5.3-6.1 g of ammonium bicarbonate and 6.6-7.3 g of sodium hydroxide to 350 mL of pure water and stir to form solution A;

[0019] (2) Immerse the alumina fiber mesh in solution A and place it in an ultrasonic cleaner for 30 minutes.

[0020] A flexible mesh water treatment material is prepared by the above method. The flexible mesh water treatment material is coated with a gallium-tungsten-cerium ternary composite oxide active coating on an activated alumina fiber mesh, and the active coating accounts for 7.5% to 8.8% of the mass percentage of the flexible mesh water treatment material.

[0021] Furthermore, the gallium-tungsten-cerium ternary composite oxide active coating is composed of three oxides: gallium oxide, tungsten oxide and cerium oxide. The ratio of the three oxides is determined by the raw material composition, which is the key to the flexible mesh water treatment material maintaining high stability and water treatment activity.

[0022] Furthermore, the flexible mesh water treatment material maintains stable structure and performance at temperatures below 550°C.

[0023] Compared with the prior art, the advantages of the present invention are:

[0024] (1) By optimizing the raw materials and preparation process, a gallium-tungsten-cerium ternary composite oxide active coating with photocatalytic purification activity was prepared on the activated alumina fiber mesh. The coating has a strong bonding force with the activated alumina fiber mesh, good compatibility, and no adverse effects on each other.

[0025] (2) The preparation process of the present invention plays an important role in forming a high-performance flexible mesh water treatment material, such as the activation of the alumina fiber mesh and the fiber mesh coating steps are key factors.

[0026] (3) The composition and structure of the gallium-tungsten-cerium ternary composite oxide active coating in the present invention are key elements to ensure the water treatment activity and stability of the flexible mesh water treatment material, and have important innovative significance. The prepared flexible mesh water treatment material retains the strength, corrosion resistance and flexibility of the alumina fiber mesh, and at the same time has the ability to decompose and purify organic pollutants in water under light. The organic matter adsorbed on the flexible mesh water treatment material can be decomposed under light. The flexible mesh water treatment material can be used for continuous purification of organic pollutants in wastewater. The flexible mesh water treatment material can be widely used for the removal and purification of various organic pollutants in water. DETAILED DESCRIPTION

[0027] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only intended to illustrate the present invention and are not intended to limit the scope of the present invention. The operating methods in the following examples where no specific conditions are indicated are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0028] The various chemical raw materials are all pure materials.

[0029] Example 1

[0030] A method for preparing a flexible mesh water treatment material comprises the following process steps:

[0031] Step 1: Activation of Alumina Fiber Mesh

[0032] (1) Add 5.3 g of ammonium bicarbonate and 6.6 g of sodium hydroxide to 350 mL of pure water and stir to form solution A;

[0033] (2) Immerse the alumina fiber mesh in solution A and place it in an ultrasonic cleaning machine for 30 minutes;

[0034] (3) The treated alumina fiber mesh was dried at 150°C for 10 h, and then calcined at 580°C for 2 h to obtain an activated alumina fiber mesh.

[0035] Step 2: Prepare Gallium-Tungsten-Cerium Precursor

[0036] (1) Add 105 mL of ethanol, 5.5 mL of isopropanol, and 3.2 g of polyethylene glycol with a molecular weight of 10,000 to a beaker in sequence and stir to form solution B;

[0037] (2) Add 235 mL of pure water, 7.2 g of gallium nitrate, 5.7 g of sodium tungstate, and 4.3 g of cerium nitrate hexahydrate into a beaker and stir to form a solution C;

[0038] (3) Add 3.5 g of octadecyltrimethylammonium chloride to solution C and stir to form solution D;

[0039] (4) Solution B and solution D were mixed, placed in a constant temperature water bath at 85° C. and stirred for 30 min to obtain a gallium-tungsten-cerium precursor.

[0040] Step 3: Fiber Mesh Lamination

[0041] (1) immersing the activated alumina fiber mesh obtained in step 1 into a gallium-tungsten-cerium precursor, keeping it in a constant temperature water bath at 85° C. for 30 min, and then taking it out and washing it with pure water;

[0042] (2) The fiber web was dried at 150°C for 10 h, and then calcined at 550°C for 2 h to obtain a flexible mesh water treatment material.

[0043] Embodiment 2 A method for preparing a flexible mesh water treatment material comprises the following process steps:

[0044] Step 1: Activation of Alumina Fiber Mesh

[0045] (1) Add 5.4 g of ammonium bicarbonate and 6.7 g of sodium hydroxide to 350 mL of pure water and stir to form solution A;

[0046] (2) Immerse the alumina fiber mesh in solution A and place it in an ultrasonic cleaning machine for 30 minutes;

[0047] (3) The treated alumina fiber mesh was dried at 150°C for 10 h, and then calcined at 590°C for 2 h to obtain an activated alumina fiber mesh.

[0048] Step 2: Prepare Gallium-Tungsten-Cerium Precursor

[0049] (1) Add 110 mL of ethanol, 5.7 mL of isopropanol, and 3.3 g of polyethylene glycol with a molecular weight of 10,000 to a beaker in sequence and stir to form solution B;

[0050] (2) Add 237 mL of pure water, 7.4 g of gallium nitrate, 5.8 g of sodium tungstate, and 4.35 g of cerium nitrate hexahydrate into a beaker and stir to form a solution C;

[0051] (3) Add 3.6 g of octadecyltrimethylammonium chloride to solution C and stir to form solution D;

[0052] (4) Solution B and solution D were mixed, placed in a constant temperature water bath at 85° C. and stirred for 30 min to obtain a gallium-tungsten-cerium precursor.

[0053] Step 3: Fiber Mesh Lamination

[0054] (1) immersing the activated alumina fiber mesh obtained in step 1 into a gallium-tungsten-cerium precursor, keeping it in a constant temperature water bath at 85° C. for 30 min, and then taking it out and washing it with pure water;

[0055] (2) The fiber web was dried at 150°C for 10 h, and then calcined at 560°C for 2 h to obtain a flexible mesh water treatment material.

[0056] Example 3 A method for preparing a flexible mesh water treatment material comprises the following process steps:

[0057] Step 1: Activation of Alumina Fiber Mesh

[0058] (1) Add 5.7 g of ammonium bicarbonate and 6.9 g of sodium hydroxide to 350 mL of pure water and stir to form solution A;

[0059] (2) Immerse the alumina fiber mesh in solution A and place it in an ultrasonic cleaning machine for 30 minutes;

[0060] (3) The treated alumina fiber mesh was dried at 150°C for 10 h, and then calcined at 590°C for 2 h to obtain an activated alumina fiber mesh.

[0061] Step 2: Prepare Gallium-Tungsten-Cerium Precursor

[0062] (1) Add 115 mL of ethanol, 5.9 mL of isopropanol, and 3.5 g of polyethylene glycol with a molecular weight of 10,000 to a beaker in sequence and stir to form solution B;

[0063] (2) Add 240 mL of pure water, 7.7 g of gallium nitrate, 5.9 g of sodium tungstate, and 4.5 g of cerium nitrate hexahydrate into a beaker and stir to form a solution C;

[0064] (3) Add 3.7 g of octadecyltrimethylammonium chloride to solution C and stir to form solution D;

[0065] (4) Solution B and solution D were mixed, placed in a constant temperature water bath at 85° C. and stirred for 30 min to obtain a gallium-tungsten-cerium precursor.

[0066] Step 3: Fiber Mesh Lamination

[0067] (1) immersing the activated alumina fiber mesh obtained in step 1 into a gallium-tungsten-cerium precursor, keeping it in a constant temperature water bath at 85° C. for 30 min, and then taking it out and washing it with pure water;

[0068] (2) The fiber web was dried at 150°C for 10 h, and then calcined at 560°C for 2 h to obtain a flexible mesh water treatment material.

[0069] Example 4 A method for preparing a flexible mesh water treatment material comprises the following process steps:

[0070] Step 1: Activation of Alumina Fiber Mesh

[0071] (1) Add 5.9 g of ammonium bicarbonate and 7.2 g of sodium hydroxide to 350 mL of pure water and stir to form solution A;

[0072] (2) Immerse the alumina fiber mesh in solution A and place it in an ultrasonic cleaning machine for 30 minutes;

[0073] (3) The treated alumina fiber mesh was dried at 150°C for 10 h, and then calcined at 600°C for 2 h to obtain an activated alumina fiber mesh.

[0074] Step 2: Prepare Gallium-Tungsten-Cerium Precursor

[0075] (1) Add 130 mL of ethanol, 6.1 mL of isopropanol, and 3.7 g of polyethylene glycol with a molecular weight of 10,000 to a beaker in sequence and stir to form solution B;

[0076] (2) Add 242 mL of pure water, 8.0 g of gallium nitrate, 6.0 g of sodium tungstate, and 4.5 g of cerium nitrate hexahydrate into a beaker and stir to form a solution C;

[0077] (3) Add 3.8 g of octadecyltrimethylammonium chloride to solution C and stir to form solution D;

[0078] (4) Solution B and solution D were mixed, placed in a constant temperature water bath at 85° C. and stirred for 30 min to obtain a gallium-tungsten-cerium precursor.

[0079] Step 3: Fiber Mesh Lamination

[0080] (1) immersing the activated alumina fiber mesh obtained in step 1 into a gallium-tungsten-cerium precursor, keeping it in a constant temperature water bath at 85° C. for 30 min, and then taking it out and washing it with pure water;

[0081] (2) The fiber web was dried at 150° C. for 10 h, and then calcined at 570° C. for 2 h to obtain a flexible mesh water treatment material.

[0082] Example 5 A method for preparing a flexible mesh water treatment material comprises the following process steps:

[0083] Step 1: Activation of Alumina Fiber Mesh

[0084] (1) Add 6.1 g of ammonium bicarbonate and 7.3 g of sodium hydroxide to 350 mL of pure water and stir to form solution A;

[0085] (2) Immerse the alumina fiber mesh in solution A and place it in an ultrasonic cleaning machine for 30 minutes;

[0086] (3) The treated alumina fiber mesh was dried at 150°C for 10 h, and then calcined at 600°C for 2 h to obtain an activated alumina fiber mesh.

[0087] Step 2: Prepare Gallium-Tungsten-Cerium Precursor

[0088] (1) Add 135 mL of ethanol, 6.3 mL of isopropanol, and 3.8 g of polyethylene glycol with a molecular weight of 10,000 to a beaker in sequence and stir to form solution B;

[0089] (2) Add 245 mL of pure water, 8.3 g of gallium nitrate, 6.2 g of sodium tungstate, and 4.6 g of cerium nitrate hexahydrate into a beaker and stir to form a solution C;

[0090] (3) Add 3.9 g of octadecyltrimethylammonium chloride to solution C and stir to form solution D;

[0091] (4) Solution B and solution D were mixed, placed in a constant temperature water bath at 85° C. and stirred for 30 min to obtain a gallium-tungsten-cerium precursor.

[0092] Step 3: Fiber Mesh Lamination

[0093] (1) immersing the activated alumina fiber mesh obtained in step 1 into a gallium-tungsten-cerium precursor, keeping it in a constant temperature water bath at 85° C. for 30 min, and then taking it out and washing it with pure water;

[0094] (2) The fiber web was dried at 150° C. for 10 h, and then calcined at 570° C. for 2 h to obtain a flexible mesh water treatment material.

[0095] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing a flexible mesh water treatment material, characterized in that: The process includes the following steps: Step 1: Activation of Alumina Fiber Mesh The treated alumina fiber mesh was dried at 150° C. for 10 h, and then calcined at 580-600° C. for 2 h to obtain an activated alumina fiber mesh; Step 2: Prepare Gallium-Tungsten-Cerium Precursor (1) Add 105-135 mL of ethanol, 5.5-6.3 mL of isopropanol, and 3.2-3.8 g of polyethylene glycol with a molecular weight of 10,000 to a beaker in sequence and stir to form solution B; (2) Add 235-245 mL of pure water, 7.2-8.3 g of gallium nitrate, 5.7-6.2 g of sodium tungstate, and 4.3-4.6 g of cerium nitrate hexahydrate into a beaker and stir to form a solution C; (3) Add 3.5-3.9 g of octadecyltrimethylammonium chloride to solution C and stir to form solution D; (4) mixing solution B and solution D, placing in a constant temperature water bath at 85° C. and stirring for 30 min to prepare a gallium-tungsten-cerium precursor; Step 3: Fiber Mesh Lamination (1) immersing the activated alumina fiber mesh obtained in step 1 into a gallium-tungsten-cerium precursor, keeping it in a constant temperature water bath at 85° C. for 30 min, and then taking it out and washing it with pure water; (2) The cleaned fiber web is dried at 150° C. for 10 h, and then calcined at 550-570° C. for 2 h to obtain a flexible mesh water treatment material.

2. The method for preparing a flexible mesh water treatment material according to claim 1, characterized in that: The alumina fiber mesh described in step 1 is a square mesh woven from alumina fibers with a diameter of 1 mm. The spacing between the alumina fibers is 1.5 mm and can withstand a high temperature of 1000°C.

3. The method for preparing a flexible mesh water treatment material according to claim 1, characterized in that: The alumina fiber mesh processing process described in step 1 is as follows: (1) Add 5.3-6.1 g of ammonium bicarbonate and 6.6-7.3 g of sodium hydroxide to 350 mL of pure water and stir to form solution A; (2) Immerse the alumina fiber mesh in solution A and place it in an ultrasonic cleaner for 30 minutes.

4. A flexible mesh water treatment material, prepared by the method according to any one of claims 1 to 3, characterized in that: The flexible mesh water treatment material is coated with a gallium-tungsten-cerium ternary composite oxide active coating on an activated alumina fiber net, and the mass percentage of the active coating in the flexible mesh water treatment material is 7.5% to 8.8%.

5. A flexible mesh water treatment material according to claim 4, characterized in that: The gallium-tungsten-cerium ternary composite oxide active coating is composed of three oxides: gallium oxide, tungsten oxide and cerium oxide. The ratio of the three oxides is determined by the composition of the raw materials. This is the key to maintaining high stability and water treatment activity of the flexible mesh water treatment material.

6. A flexible mesh water treatment material according to claim 4, characterized in that: The flexible mesh water treatment material maintains stable structure and performance at temperatures below 550°C.

Citation Information

Patent Citations

  • Honeycomb shaped wire mesh carrier for purifying exhaust air

    CN101274292A

  • Self-cleaning membrane bioreactor

    CN102452771A

  • Metal net immobilization titanium dioxide photocatalyst and preparing method

    CN103127934A

  • Method for preparing two-dimensional strontium titanate meshed materials

    CN106984295A

  • Preparation method of load type photocatalytic purification net block

    CN1515352A

Cited By

  • Preparation method of self-purification cascade ring filler

    CN119263467A

  • Preparation method of self-cleaning stepped ring filler

    CN119263467B