Modified indium oxide catalyst, preparation method thereof and method for preparing methanol through carbon dioxide hydrogenation
By controlling the content of cubic phase and hexagonal phase in the indium oxide catalyst and introducing monoclinic crystal zirconia to form a mixed crystal structure, the problem of insufficient catalytic activity and stability is solved, and the effect of efficient conversion of carbon dioxide to methanol is achieved. .
Patent Information
- Application Number
- CN202310464480.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-04-26
AI Technical Summary
The existing indium oxide catalysts lack catalytic activity and stability in carbon dioxide hydrogenation reaction, resulting in low conversion rate of methanol generation and high cost.
By controlling the content of cubic phase and hexagonal phase in the indium oxide catalyst and introducing monoclinic crystal zirconia, a cubic phase/hexagonal phase mixed crystal is formed, the reaction activity and stability of the catalyst are improved and production costs are reduced.
It significantly improves the conversion rate of carbon dioxide and the selectivity of methanol, extends the service life of the catalyst, reduces production costs, and achieves efficient methanol production.
Smart Images

Figure CN118874453A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon dioxide hydrogenation catalysts, and in particular to a modified indium oxide catalyst and a preparation method thereof, and a method for preparing methanol by hydrogenating carbon dioxide. Background Art
[0002] The rapid development of the global economy has led to an increase in CO2 emissions, and the increase in carbon dioxide content in the air is an important factor causing environmental problems such as greenhouse effect and global warming. Therefore, the study of carbon dioxide emission reduction and conversion and utilization technology has become an urgent problem to be solved. Methanol is an important raw material for chemicals and a substitute for fossil fuels. The preparation of methanol by reacting CO2 with H2 from renewable energy can not only solve greenhouse gas control but also be an effective way to replace fossil fuels. Therefore, the catalytic conversion of carbon dioxide into methanol products has received more attention.
[0003] Due to the stable chemical properties of CO2 and the difficulty in activation, the conversion rate of this reaction is generally low. The production of methanol is an exothermic reaction. Thermodynamically, low temperature is conducive to methanol production but not conducive to the activation of carbon dioxide. Therefore, it is necessary to select a suitable reaction temperature and design an efficient catalyst.
[0004] At present, the catalysts widely studied for synthesizing methanol include modified copper-based catalysts, precious metal catalysts and zinc oxide catalysts. However, in the modified statistical catalytic system, the high activity of the side reaction reverse water gas shift (RWGS) and the poor stability of the H2O-induced active phase sintering limit its further application. In the precious metal catalytic system and the zinc oxide catalytic system, the high cost of precious metals and the low activity and easy migration of zinc oxide also limit the further application of such catalysts in the field of carbon dioxide catalytic hydrogenation to a certain extent. In2O3 has moderate CO2 and CO adsorption capacity, showing methanol selectivity that is significantly better than Cu, Co, and precious metal catalysts, as well as higher catalytic activity than ZnO catalysts, which has attracted widespread attention from scientific researchers. However, the catalytic effect of In2O3 catalysts in the prior art still needs to be further improved. Summary of the invention
[0005] The purpose of the present invention is to overcome the problems of insufficient catalytic activity and stability of indium oxide catalysts in the prior art, and to provide a modified indium oxide catalyst and a preparation method thereof, and a method for preparing methanol by hydrogenating carbon dioxide. The modified indium oxide catalyst has better catalytic effect and can effectively improve methanol selectivity.
[0006] In order to achieve the above-mentioned object, the first aspect of the present invention provides a modified indium oxide catalyst, the catalyst comprising indium oxide and a modifying element, the modifying element being zirconium;
[0007] The indium oxide comprises cubic indium oxide and hexagonal indium oxide, and the mass ratio of the cubic indium oxide to the hexagonal indium oxide is 1:0.1-50; the modifying element is at least partially present in the form of zirconium oxide, and the zirconium oxide has a monoclinic crystal structure.
[0008] Preferably, the mass ratio of indium to zirconium, calculated as oxide, is 1-6:1, preferably 1.5-3:1.
[0009] A second aspect of the present invention provides a method for preparing a modified indium oxide catalyst, the method comprising:
[0010] (1) mixing an indium salt, a first precipitant and a modifier to obtain a precipitation mother solution;
[0011] Wherein, the modifier is zirconium oxide having a monoclinic crystal form;
[0012] (2) aging the precipitation mother solution;
[0013] The aging conditions include: temperature of 120-200°C and time of 8-48h;
[0014] (3) The product obtained in step (2) is subjected to solid-liquid separation, followed by drying and roasting.
[0015] The third aspect of the present invention provides a modified indium oxide catalyst obtained by the above preparation method.
[0016] The fourth aspect of the present invention provides a method for preparing methanol by hydrogenating carbon dioxide, the method comprising: contacting carbon dioxide and hydrogen in the presence of a catalyst under carbon dioxide hydrogenation conditions; the catalyst is the modified indium oxide catalyst described in the first aspect or the third aspect.
[0017] In the prior art, the indium oxide in the indium oxide catalyst generally has a cubic crystal structure, such as the supported indium oxide catalysts disclosed in US20200061582A1 and US20210322957A1; in addition, CN110479235A discloses a hexagonal indium oxide with a nano-multilevel structure, but the CO2 conversion rate is low.
[0018] The inventors of the present invention have found in their research that by controlling the content of cubic indium oxide and hexagonal indium oxide in the indium oxide catalyst, under the synergistic effect of monoclinic zirconium oxide, the reaction activity of the catalyst can be improved, the reaction stability is good, and the catalyst deactivation rate is low.
[0019] The preparation method of the modified indium oxide catalyst provided by the present invention can effectively control the crystal orientation of indium oxide by controlling the reaction conditions and introducing monoclinic zirconium oxide, and simply control the content of cubic indium oxide and hexagonal indium oxide in the catalyst. The process steps are simple, the production cost can be effectively reduced, and mass production can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is the XRD pattern of the catalyst prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0021] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0022] The first aspect of the present invention provides a modified indium oxide catalyst, the catalyst comprising indium oxide and a modifying element, the modifying element being zirconium;
[0023] The indium oxide comprises cubic indium oxide and hexagonal indium oxide, and the mass ratio of the cubic indium oxide to the hexagonal indium oxide is 1:0.1-50; the modifying element is at least partially present in the form of zirconium oxide, and the zirconium oxide has a monoclinic crystal structure.
[0024] The inventors of the present invention have found in their research that cubic indium oxide has excellent CO2 activation ability and a strong reverse water gas reaction, resulting in a low CH3OH selectivity, while hexagonal indium oxide has a high methanol selectivity and a low CO2 conversion rate. In order to make the catalyst have both high methanol selectivity and high CO2 conversion rate, the crystalline composition of indium oxide was further studied.
[0025] In the catalyst of the present invention, indium oxide is a mixed crystal material, that is, indium oxide has two crystal structures of cubic phase and hexagonal phase at the same time, and the two crystal structures are mixed phases formed by oriented crystallization in the presence of modifying elements, rather than a pure physical mixed state. The inventors found in the study that in the process of synthesizing hexagonal indium oxide, under the synergistic effect of monoclinic zirconium oxide, cubic phase / hexagonal phase indium oxide mixed crystals can be formed, so that the catalyst can improve the CO2 conversion rate of the catalyst while maintaining high methanol selectivity, can improve the reaction activity of the catalyst, has good reaction stability, and has a low catalyst deactivation rate.
[0026] In the present invention, the crystal morphology of each component in the catalyst is characterized by an X-ray diffraction method. In the X-ray diffraction pattern of the standard cubic indium oxide, characteristic diffraction peaks are present at 2θ of 21.5°, 30.6°, 35.5°, 51.0°, and 60.7°, which correspond to the (211), (222), (400), (440), and (622) crystal planes of cubic indium oxide, respectively (JCPDS 06-0416); in the X-ray diffraction pattern of the standard hexagonal indium oxide, characteristic diffraction peaks are present at 2θ of 22.4°, 31.0°, 32.6°, and 45.7°, which belong to the (012), (104), (110), and (024) crystal planes of hexagonal indium oxide, respectively (JCPDS 22-0336). The content of each crystal form of indium oxide is further calculated by the formula Wc(%)=[Ac / (Ac+3.4Ah)]×100%. Wherein, Ac and Ah represent the fitting intensity (fitting peak area) of c-In2O3(222) crystal plane and h-In2O3(104) crystal plane respectively, and the constant coefficient 3.4 is the fitting intensity ratio of the two peaks, which can be obtained through preliminary XRD experiments.
[0027] In the present invention, preferably, the mass ratio of the cubic indium oxide to the hexagonal indium oxide is 1:0.5-20. For example, it can be 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19, 1:20 and other limited but non-limiting ratios. Controlling the ratio of the cubic indium oxide to the hexagonal indium oxide in the catalyst within the above preferred range can take into account both high methanol selectivity and high CO2 conversion rate.
[0028] According to the present invention, it can be determined from the X-ray diffraction pattern of the catalyst that the modifying element is at least partially present in the form of zirconium oxide, and the zirconium oxide has a monoclinic crystalline form. The inventors of the present invention have found in their research that the monoclinic zirconium oxide in the catalyst helps to stabilize the indium oxide crystalline form, and at the same time, the catalytic activity and stability of the catalyst can be further improved through the synergistic effect of monoclinic zirconium oxide, cubic indium oxide and hexagonal indium oxide.
[0029] The present invention has a wide selection range for the content of indium and zirconium in the catalyst. Preferably, based on the total weight of the catalyst, the content of indium is 40-90wt%, preferably 60-80wt% in terms of oxide; the content of zirconium is 10-60wt%, preferably 20-40wt%. For example, calculated as oxide, the indium content can be 60wt%, 61wt%, 62wt%, 63wt%, 64wt%, 65wt%, 66wt%, 67wt%, 68wt%, 69wt%, 70wt%, 71wt%, 72wt%, 73wt%, 74wt%, 75wt%, 76wt%, 77wt%, 78wt%, 79wt%, 80wt% and the like typical but non-limiting contents; calculated as oxide, the zirconium content can be 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt%, 40wt% and the like typical but non-limiting contents.
[0030] In the present invention, the contents of indium oxide and zirconium oxide are measured by XRF method.
[0031] In the present invention, it is not excluded that part of the modifying elements exist in the form of indium / zirconium oxide.
[0032] In the prior art, zirconium oxide is more often used as a catalyst carrier, such as the supported indium oxide catalyst disclosed in US20200061582A1 and US20210322957A1, in which zirconium oxide has a high crystallinity and a content much higher than that of indium oxide, because the zirconium oxide carrier plays a role in dispersing indium oxide. However, in the present invention, zirconium exists as a modifying element, and the content of zirconium oxide in the catalyst is preferably not higher than that of indium oxide.
[0033] In a further preferred embodiment, in the modified indium oxide catalyst, the mass ratio of indium to zirconium, calculated as oxide, is 1-6:1, for example, it can be 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1 and other typical but non-limiting ratios. Preferably, the mass ratio of indium to zirconium, calculated as oxide, is 1.5-3:1. In the above preferred case, it is conducive to the formation of cubic indium oxide in the preparation of hexagonal indium oxide.
[0034] A second aspect of the present invention provides a method for preparing a modified indium oxide catalyst, the method comprising:
[0035] (1) mixing an indium salt, a first precipitant and a modifier to obtain a precipitation mother solution;
[0036] Wherein, the modifier is zirconium oxide having a monoclinic crystal form;
[0037] (2) aging the precipitation mother solution;
[0038] The aging conditions include: temperature of 120-200°C and time of 8-48h;
[0039] (3) The product obtained in step (2) is subjected to solid-liquid separation, followed by drying and roasting.
[0040] The inventors of the present invention have discovered in their research that, during the aging process of the precipitation mother solution, monoclinic zirconium oxide can induce the crystal orientation of indium oxide, so that the catalyst contains both cubic indium oxide and hexagonal indium oxide, forming cubic / hexagonal indium oxide mixed crystals; and the monoclinic zirconium oxide helps to regulate the oxygen vacancy concentration in the catalyst, further improving the catalytic activity and stability of the catalyst.
[0041] The present invention has a wide range of selection for the amount of indium salt and modifier. Preferably, the amount of indium salt and modifier is such that, based on the total weight of the prepared catalyst, the content of indium is 40-90wt%, preferably 60-80wt% in terms of oxide; the content of zirconium is 10-60wt%, preferably 20-40wt%; for example, in terms of oxide, the content of indium can be 60wt%, 61wt%, 62wt%, 63wt%, 64wt%, 65wt%, 66wt%, 67wt%, 68wt%, 69wt%, 70wt%, 71wt%, 72wt%, 73wt%, 74wt% %, 75wt%, 76wt%, 77wt%, 78wt%, 79wt%, 80wt% or other typical but non-limiting contents or ranges therebetween; calculated as oxide, the zirconium content may be 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt%, 40wt% or other typical but non-limiting contents or ranges therebetween.
[0042] In a further preferred embodiment, the mass ratio of the indium salt to the modifier calculated as oxide is 1-6:1, for example, it can be 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1, etc. typical but non-limiting ratios or ranges therebetween. Preferably, the mass ratio of the indium salt to the modifier calculated as oxide is 1.5-3:1.
[0043] According to a preferred embodiment of the present invention, the mixing in step (1) is carried out under stirring conditions. The present invention has no particular limitation on the stirring conditions, as long as the components can be fully dispersed. Preferably, the mixing temperature is 20-50°C and the mixing time is 1-10h.
[0044] The present invention has no particular limitation on the order of the mixing. The indium salt, the first precipitant and the modifier may be added to the reactor together for mixing, or the indium salt and the first precipitant may be mixed and then the modifier may be added. In a further preferred embodiment, the mixing in step (1) includes: first mixing the indium salt and the precipitant and then mixing the modifier. The above preferred embodiment is advantageous for forming an appropriate amount of cubic indium oxide and hexagonal indium oxide, thereby improving the methanol selectivity and CO2 conversion rate of the catalyst.
[0045] According to the present invention, preferably, the precipitation mother solution further contains a solvent, and the solvent is an organic solvent and / or water. Further preferably, the solvent is a mixture of an organic solvent and water, and the volume ratio of the organic solvent to water is preferably 1-5:1.
[0046] In the present invention, the organic solvent may be an alcohol and / or amide solvent. Preferably, the organic solvent is selected from at least one of ethanol, methanol, isopropanol, ethylene glycol, triethylene glycol and N,N-dimethylacetamide.
[0047] According to a particularly preferred embodiment of the present invention, the solvent is a mixture of ethanol and water, and the volume ratio of ethanol to water is 1-3:1.
[0048] The present invention has no particular limitation on the timing of introducing the solvent. The indium salt and the first precipitant may be added to the solvent to obtain an indium salt solution and a first precipitant solution, respectively, and then the mixing described in step (1) is performed. Alternatively, the indium salt, the first precipitant and the modifier may be mixed and then the solvent may be added for dispersion.
[0049] In a further preferred embodiment, the indium salt is provided in the form of an indium salt solution, and the concentration of the indium salt solution is 0.1-0.8 mol / L.
[0050] The present invention has a wide range of selection for the specific type of the indium salt. As long as the indium element can be provided, any conventional soluble indium salt in the art can be used in the present invention. For example, the indium salt can be selected from at least one of indium nitrate, indium chloride and indium sulfate. The indium salt may also contain crystal water, which is well known to those skilled in the art and will not be described in detail here.
[0051] Preferably, the first precipitant is provided in the form of a first precipitant solution, and the concentration of the first precipitant solution is 1-2 mol / L.
[0052] In the present invention, the compositions of the solvents in the indium salt solution and the first precipitant solution may be the same or different, and both satisfy the above-mentioned definition range of the solvent composition.
[0053] Preferably, the first precipitant is selected from at least one of urea, aqueous ammonia, (NH4)2CO3, Na2CO3 and NaOH.
[0054] According to the present invention, preferably, the molar ratio of the amount of the first precipitant to the indium salt calculated as indium element is 5-8:1, for example, it can be 5:1, 5.2:1, 5.4:1, 5.6:1, 5.8:1, 6:1, 6.2:1, 6.4:1, 6.6:1, 6.8:1, 7:1, 7.2:1, 7.4:1, 7.6:1, 7.8:1, 8:1 and other typical but non-limiting ratios. Preferably, the molar ratio of the amount of the first precipitant to the indium salt calculated as indium element is 6-7:1.
[0055] In the present invention, the modifier is monoclinic zirconium oxide. The present invention has no particular limitation on the source of the modifier, which can be purchased commercially or prepared by any method known in the art.
[0056] In a specific embodiment of the present invention, the preparation method of the modifier comprises: mixing a zirconium source and a second precipitant, performing a hydrothermal reaction at 120-200° C. for 15-25 hours, and then drying and calcining the product obtained by the hydrothermal reaction.
[0057] According to a preferred embodiment of the present invention, the drying temperature is 80-150° C. and the drying time is 15-25 hours.
[0058] According to a preferred embodiment of the present invention, the calcination temperature is 400-600° C. and the calcination time is 3-6 hours.
[0059] The present invention has a wide range of selection for the specific type of the zirconium source, as long as it can provide zirconium element, for example, zirconium nitrate and / or zirconium oxynitrate. The zirconium source may also contain crystal water, which is well known to those skilled in the art and will not be described in detail here.
[0060] In the present invention, the second precipitant and the first precipitant have the same selection range, and their specific selections may be the same or different, and the present invention has no particular limitation on this.
[0061] Preferably, the molar ratio of the amount of the second precipitant to the zirconium source calculated as zirconium element is 4-11:1, preferably 4.5-10:1.
[0062] According to the present invention, preferably, in step (2), the aging conditions include: a temperature of 120-150°C, for example, typical but not limiting aging temperatures such as 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, etc. The aging time is preferably 16-20h, for example, typical but not limiting times such as 16h, 17h, 18h, 19h, 20h, etc. By controlling the aging temperature and time, it is beneficial to the formation of cubic indium oxide in hexagonal indium oxide, but too long an aging time may result in an excessive content of cubic indium oxide.
[0063] In a specific embodiment of the present invention, step (2) further comprises: washing and solid-liquid separation of the product obtained by aging. The washing and solid-liquid separation can be performed using conventional operations and conditions in the art, for example, deionized water can be used for the washing. The solid-liquid separation can be performed by centrifugation.
[0064] According to the present invention, preferably, in step (3), the drying conditions include: temperature of 50-100°C, preferably 60-80°C; time of 12-25h, preferably 14-22h.
[0065] Preferably, in step (3), the calcination conditions include: a temperature of 350-600°C, for example, 350°C, 360°C, 370°C, 380°C, 390°C, preferably 400-500°C; and a calcination time of 1-8h, preferably 3-6h.
[0066] In a specific embodiment of the present invention, step (3) further comprises: molding and screening the product obtained by the calcination. The present invention has no particular limitation on the molding method, and those skilled in the art can select it according to actual needs, for example, tableting can be used.
[0067] The third aspect of the present invention provides a modified indium oxide catalyst obtained by the above preparation method.
[0068] The fourth aspect of the present invention provides a method for preparing methanol by hydrogenating carbon dioxide, the method comprising: contacting carbon dioxide and hydrogen in the presence of a catalyst under carbon dioxide hydrogenation conditions; the catalyst is the modified indium oxide catalyst described in the first aspect or the third aspect.
[0069] According to the present invention, preferably, the carbon dioxide hydrogenation conditions include: reaction temperature of 200-400°C, reaction pressure of 1-6MPa, volume space velocity of 4500-18000h -1 , the H2 / CO2 molar ratio is 1-6; further preferably, the carbon dioxide hydrogenation conditions include: reaction temperature is 240-280°C, reaction pressure is 3-5MPa, volume space velocity is 8000-12000h -1 , the H2 / CO2 molar ratio is 3-6.
[0070] Preferably, before the contacting, the method further comprises: reducing and activating the catalyst under normal pressure and in a hydrogen atmosphere. The conditions for the reduction and activation include: a reduction temperature of 150-250° C., preferably 180-220° C., and a time of 1-4 h, preferably 1.5-3 h.
[0071] The hydrogen atmosphere may be provided by hydrogen or a mixture of hydrogen and an inert gas. Preferably, the hydrogen atmosphere is provided by a mixture of hydrogen and an inert gas, and the volume fraction of hydrogen in the mixture is 10%-50%.
[0072] The present invention will be described in detail below through examples.
[0073] In the following examples, all raw materials were purchased from Sinopharm Group.
[0074] The physical structure, cubic indium oxide content and hexagonal indium oxide content in the catalyst were obtained by X-ray diffractometer testing. In the X-ray diffraction pattern of standard cubic indium oxide, characteristic diffraction peaks are found at 2θ of 21.5°, 30.6°, 35.5°, 51.0° and 60.7°, which correspond to the (211), (222), (400), (440) and (622) crystal planes of cubic indium oxide (JCPDS06-0416), respectively; in the X-ray diffraction pattern of standard hexagonal indium oxide, characteristic diffraction peaks are found at 2θ of 22.4°, 31.0°, 32.6° and 45.7°, which belong to the (012), (104), (110) and (024) crystal planes of hexagonal indium oxide (JCPDS 22-0336), respectively. The content of each crystal form of indium oxide is further calculated by the formula Wc(%)=[Ac / (Ac+3.4Ah)]×100%. Wherein, Ac and Ah represent the fitting intensity (fitting peak area) of c-In2O3(222) crystal plane and h-In2O3(104) crystal plane respectively, and the constant coefficient 3.4 is the fitting intensity ratio of the two peaks, which can be obtained through preliminary XRD experiments.
[0075] The contents of indium oxide and zirconium oxide in the catalyst were tested by XRF method.
[0076] The product composition of the reaction of preparing methanol by hydrogenation of carbon dioxide was analyzed using a gas chromatograph purchased from Agilent Technologies (China) Co., Ltd.
[0077] Example 1
[0078] (1) Dissolve 9.53 g of ZrO(NO3)2·2H2O in deionized water to 100 mL and stir to dissolve. Then weigh 20.67 g of urea and add it to the above solution and continue stirring to dissolve. After dissolution, pour it into a hydrothermal kettle, seal it and place it in an oven for hydrothermal reaction at 180°C for 20 hours. After the hydrothermal reaction is completed, cool it naturally to room temperature. Open the hydrothermal kettle, filter and wash the hydrothermal product. Then place it in an oven and dry it at 120°C for 15 hours. Finally, calcine it at 400°C in a muffle furnace for 3 hours to obtain monoclinic ZrO2;
[0079] (2) adding 7.6 g of In(NO3)3·4H2O to a mixture of 50 mL of anhydrous ethanol and 25 mL of deionized water to obtain a solution containing a metal indium salt, adding 8 g of urea to a mixture of 60 mL of anhydrous ethanol and 20 mL of deionized water to obtain a precipitant solution, adding the precipitant solution dropwise to the solution containing the metal indium salt at 30°C, then adding 1.2 g of the monoclinic ZrO2 obtained in step (1), and stirring the mixture at a speed of 200 rpm for 4 h to obtain a precipitation mother solution;
[0080] (3) adding the precipitation mother solution obtained in step (2) into a 100 mL polytetrafluoroethylene-lined hydrothermal synthesis reactor, placing the reactor in a forced air drying oven for aging at 120° C. for 18 h to form a precipitate;
[0081] (4) The product obtained in step (3) was cooled to room temperature naturally and then centrifuged. The centrifugal precipitate was washed with deionized water until the pH value was 8, and then dried at 60° C. for 15 h, and then calcined at 380° C. for 3 h to obtain catalyst S1, which was pressed into tablets and sieved into 40-60 mesh.
[0082] The X-ray diffraction pattern of catalyst S1 is as follows: Figure 1 As shown, at 2θ of 21.5°, 30.6°, 35.5°, 51.0°, and 60.7°, there are characteristic diffraction peaks of cubic indium oxide, and at 2θ of 22.4°, 31.0°, 32.6°, and 45.7°, there are characteristic diffraction peaks of hexagonal indium oxide, proving that the catalyst contains cubic indium oxide and hexagonal indium oxide. At the same time, at 2θ of 30.3°, there is a characteristic peak of monoclinic zirconium oxide, proving that the zirconium in the catalyst exists at least partially in the form of monoclinic zirconium oxide. The content of each component in the catalyst is shown in Table 1.
[0083] Example 2
[0084] (1) Weigh 6.23g of ZrO(NO3)2·2H2O, dissolve it to 60mL with deionized water, and stir to dissolve. Then weigh 10.03g of urea and add it to the above solution and continue to stir and dissolve. After dissolution, pour it into a 100mL hydrothermal kettle, seal it and place it in an oven at 160℃ for 18h. After the hydrothermal reaction is completed, cool it naturally to room temperature. Open the hydrothermal kettle, filter and wash the hydrothermal product. Then place it in an oven at 110℃ and dry it for 12h. Finally, calcine it at 450℃ in a muffle furnace for 3h to obtain monoclinic ZrO2;
[0085] (2) adding 7.3 g of In(NO3)3·4H2O to a mixture of 80 mL of anhydrous ethanol and 40 mL of deionized water to obtain a solution containing a metal indium salt, adding 9.2 g of urea to a mixture of 80 mL of anhydrous ethanol and 30 mL of deionized water to obtain a precipitant solution, adding the precipitant solution dropwise to the solution containing the metal indium salt at 30°C, then adding 1.0 g of the monoclinic ZrO2 obtained in step (1), and stirring at a speed of 150 rpm for 7 h to obtain a precipitation mother solution;
[0086] (3) adding the precipitation mother solution obtained in step (2) into a 100 mL polytetrafluoroethylene-lined hydrothermal synthesis reactor, placing the reactor in a forced air drying oven for aging at a temperature of 130° C. for 48 h to form a precipitate;
[0087] (4) The product obtained in step (3) was naturally cooled to room temperature and then centrifuged. The centrifugal precipitate was washed with deionized water until the pH value was 7, and then dried at 80°C for 12 hours, and then calcined at 450°C for 3 hours. The pellets were sieved into 40-60 mesh to obtain catalyst S2 (the contents of its components are shown in Table 1).
[0088] Example 3
[0089] (1) Weigh 6.68g of ZrO(NO3)2·2H2O, dissolve it to 50mL with deionized water, and stir to dissolve. Then weigh 8.67g of urea and add it to the above solution and continue to stir to dissolve. After dissolution, pour it into a 100mL hydrothermal kettle, seal it and place it in an oven for hydrothermal reaction at 190℃ for 15h. After the hydrothermal reaction is completed, cool it naturally to room temperature. Open the hydrothermal kettle, filter and wash the hydrothermal product. Then place it in an oven at 100℃ and dry it for 15h. Finally, calcine it at 500℃ in a muffle furnace for 4h to obtain monoclinic ZrO2;
[0090] (2) adding 8.5 g of In(NO3)3·4H2O to a mixture of 40 mL of anhydrous ethanol and 24 mL of deionized water to obtain a solution containing a metal indium salt, adding 8 g of urea to a mixture of 40 mL of anhydrous ethanol and 10 mL of deionized water to obtain a precipitant solution, adding the precipitant solution dropwise to the solution containing the metal indium salt at 30°C, then adding 2 g of the monoclinic ZrO2 obtained in step (1), and stirring the mixture at a speed of 150 rpm for 6 h to obtain a precipitation mother solution;
[0091] (3) adding the precipitation mother solution obtained in step (2) into a 100 mL polytetrafluoroethylene-lined hydrothermal synthesis reactor, placing the reactor in a forced air drying oven for aging at a temperature of 120° C. for 16 h to form a precipitate;
[0092] (4) The product obtained in step (2) was cooled to room temperature naturally and then centrifuged. The centrifugal precipitate was washed with deionized water until the pH value was 7, and then dried at 60°C for 20 hours, and then calcined at 350°C for 3 hours. The pellets were sieved to 40-60 mesh to obtain catalyst S3 (the contents of its components are shown in Table 1).
[0093] Example 4
[0094] (1) Weigh 4.89g of ZrO(NO3)2·2H2O, dissolve it to 70mL with deionized water, and stir to dissolve. Then weigh 6.63g of urea and add it to the above solution and continue to stir and dissolve. After dissolution, pour it into a 100mL hydrothermal kettle, seal it and place it in an oven for hydrothermal reaction at 180℃ for 18h. After the hydrothermal reaction is completed, cool it naturally to room temperature. Open the hydrothermal kettle, filter and wash the hydrothermal product. Then place it in an oven at 110℃ and dry it for 16h. Finally, calcine it at 550℃ in a muffle furnace for 3h to obtain monoclinic ZrO2;
[0095] (2) adding 9.3 g of In(NO3)3·4H2O to a mixed solution of 80 mL of anhydrous ethanol and 40 mL of deionized water to obtain a solution containing a metal indium salt, adding 8 g of urea to a mixed solution of 60 mL of anhydrous ethanol and 25 mL of deionized water to dissolve and obtain a precipitant solution, adding the precipitant solution dropwise to the solution containing the metal indium salt at 30°C, then adding 1 g of the monoclinic ZrO2 obtained in step (1), and stirring at a speed of 200 rpm for 6 h to obtain a precipitation mother solution;
[0096] (3) adding the precipitation mother solution obtained in step (2) into a 100 mL polytetrafluoroethylene-lined hydrothermal synthesis reactor, placing the reactor in a forced air drying oven for aging at a temperature of 170° C. for 24 h to form a precipitate;
[0097] (4) The product obtained in step (3) was cooled to room temperature naturally and then centrifuged. The centrifugal precipitate was washed with deionized water until the pH value was 8, and then dried at 60°C for 22 hours, and then calcined at 500°C for 3 hours. The pellets were sieved into 40-60 mesh to obtain catalyst S4 (the contents of its components are shown in Table 1).
[0098] Example 5
[0099] (1) Weigh 5.06g of ZrO(NO3)2·2H2O, dissolve it to 80mL with deionized water, and stir to dissolve. Then weigh 7.23g of urea and add it to the above solution and continue to stir to dissolve. After dissolution, pour it into a 100mL hydrothermal kettle, seal it and place it in an oven at 160℃ for 18h. After the hydrothermal reaction is completed, cool it naturally to room temperature. Open the hydrothermal kettle, filter and wash the hydrothermal product. Then place it in an oven at 110℃ and dry it for 16h. Finally, calcine it at 500℃ in a muffle furnace for 3h to obtain monoclinic ZrO2;
[0100] (2) adding 5.4 g of In(NO3)3·4H2O to a mixed solution of 40 mL of anhydrous ethanol and 20 mL of deionized water to obtain a solution containing a metal indium salt, adding 6 g of urea to a mixed solution of 50 mL of anhydrous ethanol and 20 mL of deionized water, adding the precipitant solution dropwise to the solution containing the metal indium salt at 30°C, then adding 0.8 g of the monoclinic ZrO2 obtained in step (1), and stirring the mixture at a speed of 100 rpm for 6 h to obtain a precipitation mother solution;
[0101] (3) adding the precipitation mother solution obtained in step (2) into a 100 mL polytetrafluoroethylene-lined hydrothermal synthesis reactor, placing the reactor in a forced air drying oven for aging at a temperature of 150° C. for 28 h to form a precipitate;
[0102] (4) The product obtained in step (3) was cooled to room temperature and then centrifuged. The centrifugal precipitate was washed with deionized water until the pH value was 8, and then dried at 80°C for 14 h, calcined at 460°C for 3 h, pressed into tablets and sieved into 40-60 mesh to obtain catalyst S5 (the contents of its components are shown in Table 1).
[0103] Example 6
[0104] The method in Example 1 was followed, except that the amount of monoclinic ZrO2 added was 3.6 g. The prepared catalyst was denoted as S6, and the contents of its components are shown in Table 1.
[0105] Example 7
[0106] The method in Example 1 was followed, except that the amount of monoclinic ZrO2 added was 0.3 g. The catalyst obtained was denoted as S7, and the contents of its components are shown in Table 1.
[0107] Comparative Example 1
[0108] (1) adding 7.6 g of In(NO3)3·4H2O to a mixture of 50 mL of anhydrous ethanol and 25 mL of deionized water to obtain a solution containing a metal indium salt, adding 8 g of urea to a mixture of 60 mL of anhydrous ethanol and 20 mL of deionized water to obtain a precipitant solution, and adding the precipitant solution dropwise to the solution containing the metal indium salt at 30°C to obtain a precipitation mother solution;
[0109] (2) adding the precipitation mother solution obtained in step (1) into a 100 mL polytetrafluoroethylene-lined hydrothermal synthesis reactor, placing the reactor in a forced air drying oven for aging at 120° C. for 18 h to form a precipitate;
[0110] (3) The product obtained in step (2) was cooled to room temperature naturally and then centrifuged. The centrifugal precipitate was washed with deionized water until the pH value was 8, and then dried at 60° C. for 15 h. The product was calcined at 380° C. for 3 h, pressed into tablets, and sieved into 40-60 mesh to obtain catalyst DS1.
[0111] XRD test shows that catalyst DS1 contains only hexagonal indium oxide.
[0112] Comparative Example 2
[0113] (1) 7.6 g of In(NO3)3·4H2O was added to a mixture of 50 mL of anhydrous ethanol and 25 mL of deionized water to obtain a solution containing a metal indium salt, 8 g of urea was added to a mixture of 60 mL of anhydrous ethanol and 20 mL of deionized water to obtain a precipitant solution, the precipitant solution was added dropwise to the solution containing the metal indium salt at 30°C, and then 1.2 g of cubic ZrO2 (commercially available) was added, and the mixture was fully stirred at a speed of 200 rpm for 4 h to obtain a precipitation mother solution;
[0114] (2) adding the precipitation mother solution obtained in step (1) into a 100 mL polytetrafluoroethylene-lined hydrothermal synthesis reactor, placing the reactor in a forced air drying oven for aging at 120° C. for 18 h to form a precipitate;
[0115] (3) The product obtained in step (2) was cooled to room temperature and then centrifuged. The precipitate was washed with deionized water until the pH value was 8, and then dried at 60°C for 15 h. The precipitate was calcined at 380°C for 3 h, pressed into tablets and sieved into 40-60 mesh to obtain catalyst DS2 (the contents of its components are shown in Table 1).
[0116] Comparative Example 3
[0117] The method in Example 1 was followed, except that the aging temperature in step (3) was 100° C. and the aging time was 16 h. The obtained catalyst was designated as DS3.
[0118] Comparative Example 4
[0119] Commercially available cubic indium oxide and hexagonal indium oxide obtained in Comparative Example 1 were mixed and ground in a mass ratio of 1:19, and the obtained product was recorded as DS4.
[0120] Table 1
[0121]
[0122]
[0123] Evaluation of the reaction of producing methanol by hydrogenation of carbon dioxide
[0124] The catalysts prepared in the above embodiments and comparative examples were used as reaction catalysts and loaded into a stainless steel reactor with an inner diameter of 8 mm. First, 10% H2 / 90% N2 was used for reduction at 200°C for 2 h, at normal pressure, and with an atmosphere flow rate of 7 L / h. Then, carbon dioxide was hydrogenated to produce methanol. The reaction conditions were as follows: reaction pressure of 5 MPa, reaction temperature of 280°C, and raw material (carbon dioxide and hydrogen) volume space velocity of 15000 h / h. -1 , the H2 / CO2 molar ratio was 5. After 500 hours of reaction, the liquid product was collected in an ice-water bath. The product composition was analyzed by gas chromatography. The evaluation results are shown in Table 2.
[0125] Table 2
[0126]
[0127]
[0128] It can be seen from the results in Table 2 that the use of the catalyst prepared in the embodiment of the present invention to catalyze the hydrogenation of carbon dioxide can effectively improve the conversion rate of carbon dioxide and can improve the selectivity of methanol, indicating that the catalyst within the protection scope of the present invention has a good catalytic effect and a good methanol selectivity.
[0129] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A modified indium oxide catalyst, It is characterized in that The catalyst comprises indium oxide and a modifying element, wherein the modifying element is zirconium; The indium oxide comprises cubic indium oxide and hexagonal indium oxide, and the mass ratio of the cubic indium oxide to the hexagonal indium oxide is 1:0.1-50; the modifying element is at least partially present in the form of zirconium oxide, and the zirconium oxide has a monoclinic crystal structure.
2. The catalyst according to claim 1, in, The mass ratio of the cubic indium oxide to the hexagonal indium oxide is 1:0.5-20.
3. The catalyst according to claim 1 or 2, in, Based on the total weight of the catalyst, the content of indium is 40-90wt%, preferably 60-80wt% in terms of oxide; the content of zirconium is 10-60wt%, preferably 20-40wt%; Preferably, the mass ratio of indium to zirconium, calculated as oxide, is 1-6:1, preferably 1.5-3:
1.
4. A method for preparing a modified indium oxide catalyst, the method include: (1) mixing an indium salt, a first precipitant and a modifier to obtain a precipitation mother solution; Wherein, the modifier is zirconium oxide having a monoclinic crystal form; (2) aging the precipitation mother solution; The aging conditions include: temperature of 120-200°C and time of 8-48h; (3) The product obtained in step (2) is subjected to solid-liquid separation, followed by drying and roasting.
5. The preparation method according to claim 4, in, The indium salt and the modifier are used in such an amount that, based on the total weight of the prepared catalyst, the indium content is 40-90wt%, preferably 60-80wt% in terms of oxide; the zirconium content is 10-60wt%, preferably 20-40wt%; Preferably, the mass ratio of the indium salt to the modifier calculated as oxide is 1-6:1, preferably 1-3:
1.
6. The preparation method according to claim 4 or 5, in, The mixing in step (1) is carried out under stirring conditions; Preferably, the mixing in step (1) comprises: first mixing the indium salt and the precipitant, and then second mixing with the modifier; Preferably, the precipitation mother solution further contains a solvent, and the solvent is an organic solvent and / or water; Preferably, the solvent is a mixture of an organic solvent and water, and the organic solvent is preferably selected from at least one of ethanol, methanol, isopropanol, ethylene glycol, triethylene glycol and N,N-dimethylacetamide.
7. The preparation method according to any one of claims 4 to 6, in, The molar ratio of the first precipitant to the indium salt calculated as indium element is 5-8:1, preferably 6-7:1; Preferably, the indium salt is selected from at least one of indium nitrate, indium chloride and indium sulfate; Preferably, the indium salt is provided in the form of an indium salt solution, and the concentration of the indium salt solution is 0.1-0.8 mol / L; Preferably, the first precipitant is selected from urea, ammonia, (NH 4 ) 2 CO 3 、Na 2 CO 3 and at least one of NaOH; Preferably, the first precipitant is provided in the form of a first precipitant solution, and the concentration of the first precipitant solution is 1-2 mol / L.
8. The preparation method according to any one of claims 4 to 7, in, The preparation method of the modifier comprises: mixing a zirconium source and a second precipitant, performing a hydrothermal reaction at 120-200° C. for 15-25 hours, and then drying and calcining a product obtained by the hydrothermal reaction.
9. The preparation method according to any one of claims 4 to 8, in, In step (2), the aging conditions include: temperature of 120-150° C. and time of 16-28 h; Preferably, in step (3), the drying conditions include: temperature of 50-100° C., time of 12-25 h; Preferably, in step (3), the calcination conditions include: temperature of 350-600°C, preferably 400-500°C; time of 1-8h, preferably 3-6h.
10. The modified indium oxide catalyst obtained by the preparation method according to any one of claims 4 to 9.
11. A method for preparing methanol by hydrogenating carbon dioxide, the method include: contacting carbon dioxide and hydrogen in the presence of a catalyst under carbon dioxide hydrogenation conditions; The catalyst is the modified indium oxide catalyst according to any one of claims 1 to 3 and 10; Preferably, the carbon dioxide hydrogenation conditions include: reaction temperature of 200-400°C, reaction pressure of 1-6 MPa, volume space velocity of 4500-18000 h -1 , H 2 / CO 2 The molar ratio is 1-6.
Citation Information
Patent Citations
Preparation method of indium oxide with controllable crystal form
CN109205659A
Indium oxide catalyst and preparation method and application thereof
CN110479235A
Lithium-doped zirconium oxide loaded indium oxide catalyst, preparation method and applications thereof
CN110586064A
Preparation method of Zr-In spherical oxide catalyst for efficiently catalyzing CO2 hydrogenation reaction
CN112742371A
Supported indium oxide catalyst and process for methanol synthesis using the same
US20200061582A1