Method for preparing methane dry type reforming carbon-based catalyst by utilizing biogas residue pyrolysis biochar, methane dry type reforming carbon-based catalyst and application of methane dry type reforming carbon-based catalyst
By using the pyrolysis of residues of residues after anaerobic fermentation of kitchen waste, and preparing biogas dry reforming carbon-based catalysts with metal salt alcohol solution, the problems of high catalyst preparation cost and improper treatment of slag are solved, and the problem of The efficient utilization of the sterilization and the efficient catalytic activity of the catalyst promote the high added value conversion of biogas.
Patent Information
- Application Number
- CN202410921528.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-10
AI Technical Summary
The existing biogas dry reforming catalysts are costly to prepare, and the improper treatment method of the slag leads to environmental pollution, and there is a lack of effective resource utilization methods.
Biochar is prepared as a matrix by using the pyrolysis of residues of residual fermentation of kitchen waste, combined with metal salt alcohol solution for colloidal solution impregnation and calcination, and biogas dry reforming carbon-based catalyst is prepared to reduce the catalyst preparation cost and increase the catalytic efficiency.
It realizes efficient utilization of biogas slag, reduces the cost of catalyst preparation, improves the catalytic activity and stability of catalysts, and is suitable for the large-scale application of biogas dry reforming technology, and promotes the high added value conversion of biogas to downstream chemical products.
Smart Images

Figure CN118874469A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of resource utilization of biogas residues left after anaerobic fermentation of kitchen waste and high-value utilization of biogas, and specifically to a method for preparing a biogas dry reforming carbon-based catalyst by utilizing biochar from biogas residue pyrolysis, a biogas dry reforming carbon-based catalyst and applications. Background Art
[0002] In my country, kitchen waste is mostly treated by anaerobic process, which will produce a large amount of biogas residue during the treatment process, which is difficult to digest. At present, the treatment methods of biogas residue mainly include landfill, incineration, composting, land use, etc. Improper treatment of biogas residue or random discharge will cause serious eutrophication of water bodies and affect the growth of crops.
[0003] Therefore, the current biogas residue treatment methods still need to be improved. Summary of the invention
[0004] The present invention is based on the inventor's discovery and understanding of the following facts and problems:
[0005] Biogas is a gas produced by anaerobic fermentation of organic waste such as food waste and kitchen waste. Its main components are CH4 and CO2. The main ways to utilize biogas include power generation, cogeneration of heat and power, etc. At present, the second-generation resource technology that uses biogas as raw material to produce gaseous products through a catalytic process has gradually developed. Among them, biogas dry reforming is a new technology with great potential that can simultaneously convert CH4 and CO2 into synthesis gas, which is conducive to the high-value-added conversion of biogas to downstream chemical products. The current dry reforming catalyst is mainly composed of active metals and matrices. Commonly used commercial matrices such as Al2O3, SiO2, MgO, ZrO2, etc. require a large amount of organic templates in the production process, and usually use some relatively expensive surfactants, which increases the cost of catalyst preparation.
[0006] The main components of the sludge left after anaerobic fermentation of kitchen waste are undecomposed organic solids and newly formed microorganisms. It is rich in organic matter, humic acid, nitrogen, phosphorus and potassium. Among them, organic matter accounts for 30% to 50%, humic acid accounts for 10% to 20%, total nitrogen accounts for 0.8% to 2.0%, total phosphorus accounts for 0.4% to 1.2%, and total potassium accounts for 0.6% to 2.0%. The composition and properties of the sludge vary with different raw materials.
[0007] Biochar prepared by pyrolysis of biogas residue has the advantages of large specific surface area, developed porous structure, strong stability, and rich oxygen-containing functional groups. It can be used for the adsorption of pollutants such as ammonia nitrogen and phosphorus in sewage and the catalytic degradation of dyes. Biochar prepared from anaerobic biogas residue has rich alkali / alkaline earth metals and oxygen-containing functional groups, and has a high specific surface area. If biochar from pyrolysis of biogas residue can be used as a matrix to synthesize a carbon-based catalyst for biogas dry reforming, then it is possible to reduce the preparation cost of the catalyst while expanding the utilization of biogas residue, which is conducive to the large-scale application of biogas dry reforming technology. At present, there is no literature disclosing such technology at home and abroad.
[0008] In view of this, the present invention aims to alleviate or solve at least one of the above-mentioned problems to at least some extent.
[0009] In one aspect of the present invention, the present invention proposes a method for preparing a biogas dry reforming carbon-based catalyst by utilizing biogas residue pyrolysis biochar. In some embodiments of the present invention, the method for preparing a biogas dry reforming carbon-based catalyst by utilizing biogas residue pyrolysis biochar comprises the following steps: 1) drying anaerobic biogas residue from kitchen waste, crushing and screening the dried biogas residue to obtain pretreated biogas residue; 2) mixing the pretreated biogas residue with an aqueous solution of an activator, filtering and drying after immersion to obtain modified biogas residue; 3) pyrolyzing the modified biogas residue obtained in step 2) at a temperature of 500°C-800°C and in a N2 atmosphere to obtain a biogas residue biochar-based catalyst. body; 4) dissolving the biochar matrix in anhydrous ethanol to form a colloidal solution, magnetically stirring the colloidal solution at a temperature of 30°C-60°C, adding a metal salt alcohol solution dropwise for impregnation during the stirring process, and continuously stirring until the solvent is completely volatilized to obtain a catalyst powder; 5) calcining the catalyst powder at a temperature of 700°C-900°C in a N2 atmosphere, and then using a tablet press to press the calcined powder into tablets, crushing and screening to obtain a biogas dry reforming carbon-based catalyst. Using anaerobic biogas residue as a matrix to prepare a catalyst can improve the utilization rate of biogas residue; the treated biogas residue is used as a catalyst matrix for biogas dry reforming, which is conducive to reducing the preparation cost of the catalyst, and thus is conducive to the large-scale utilization of biogas dry reforming technology.
[0010] In some embodiments of the present invention, in step 4), the mass of the metal element in the alcohol solution of the added metal salt is a, the mass of the biogas residue biochar matrix in the colloidal solution is b, and the value of a / (a+b) is 5%-20%. This is conducive to improving the catalytic efficiency of the catalyst.
[0011] In some embodiments of the present invention, the metal salt includes at least one of Ni nitrate, Fe nitrate, Co nitrate, Rh nitrate and Pd nitrate; and / or, in the alcohol solution of the metal salt, the solvent includes at least one of ethanol, n-propanol, isopropanol, n-butanol and isobutanol.
[0012] In some embodiments of the present invention, the metal salt includes two of Ni nitrate, Fe nitrate, Co nitrate, Rh nitrate and Pd nitrate, and in the alcohol solution of the metal salt, the molar ratio of the two metal elements is 1:3-3:1. Thus, the prepared catalyst contains two metals, and the advantages of different metal elements complement each other, which is more conducive to improving the catalytic efficiency of the catalyst.
[0013] In some embodiments of the present invention, the activator includes at least one of KOH, ZnCl2, MgCl2, CaCl2 and FeCl3. The above activator can improve the acidity and alkalinity and / or site activity of the biogas residue biochar matrix at least to a certain extent, thereby facilitating the improvement of the catalytic efficiency of the catalyst.
[0014] In some embodiments of the present invention, in step 1), the anaerobic digestate of kitchen waste is dried at 80°C-95°C for 12-24 hours; and / or, in step 1), a 20-100 mesh sieve is used for sieving. The above conditions are used for pretreatment to obtain dry digestate with relatively uniform particles.
[0015] In some embodiments of the present invention, in step 2), the mass ratio of the pretreated biogas residue to the activator is 1:1-1:2.5; and / or, the immersion time in step 2) is 24-48 hours. This is conducive to sufficient contact between the activator and the biogas residue, thereby facilitating improvement of the performance of the substrate.
[0016] In some embodiments of the present invention, the method for preparing a biogas dry reforming carbon-based catalyst satisfies at least one of the following conditions: in step 3), the pyrolysis time is 1-3 hours; in step 4), the speed of magnetic stirring is 400r / min-800r / min; in step 5), the calcination time is 3-6 hours; the particle size of the biogas dry reforming carbon-based catalyst is 20 mesh-100 mesh.
[0017] In another aspect of the present invention, the present invention provides a biogas dry reforming carbon-based catalyst. In some embodiments of the present invention, the biogas dry reforming carbon-based catalyst is prepared using the method described above. As a result, the biogas dry reforming carbon-based catalyst has a high catalytic activity, can catalyze the biogas dry reforming reaction, convert CH4 and CO2 in the biogas into synthesis gas, and promote the high value-added conversion of biogas to downstream chemical products.
[0018] In another aspect of the present invention, the present invention proposes the application of the above-mentioned biogas dry reforming carbon-based catalyst in biogas dry reforming. The above-mentioned biogas dry reforming carbon-based catalyst is used in the biogas dry reforming process, which can play a good catalytic role, and the preparation cost of the carbon-based catalyst is low, which is conducive to the large-scale application of biogas dry reforming technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0020] Figure 1 A flow chart of a method for preparing a biogas dry reforming carbon-based catalyst by pyrolyzing biochar from biogas residue according to an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0021] The embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0022] In one aspect of the present invention, a method for preparing a biogas dry reforming carbon-based catalyst by pyrolyzing biochar from biogas residue is provided. Figure 1 The method for preparing a biogas dry reforming carbon-based catalyst by pyrolyzing biochar from biogas residue may include the following steps:
[0023] 1) Drying the anaerobic digestate from kitchen waste, crushing and screening the dried digestate to obtain pretreated digestate.
[0024] In some embodiments of the present invention, in step 1), the anaerobic digestate from kitchen waste may be dried at 80°C-95°C, and the drying time may be 12-24 hours. For example, the anaerobic digestate may be dried at 80°C, 85°C, 90°C or 95°C, and the drying time may be 12 hours, 15 hours, 18 hours, 20 hours, 24 hours, etc. Drying the anaerobic digestate under the above conditions can remove moisture and volatile impurities in the anaerobic digestate, which is beneficial to the subsequent preparation of the catalyst.
[0025] In some embodiments of the invention, the digestate may be comminuted using a plant comminutor.
[0026] In some embodiments of the present invention, in step 1), the crushed biogas residue can be screened using a 20-100 mesh sieve. For example, the biogas residue can be screened using a 20-mesh sieve, a 40-mesh sieve, a 60-mesh sieve, or a 100-mesh sieve to obtain biogas residue with smaller particles and more uniform size, so as to facilitate the subsequent loading of catalyst active substances (metal catalysts).
[0027] In step 1), the anaerobic digestate is pretreated to remove moisture from the anaerobic digestate, and the digestate is crushed and sieved to obtain digestate with uniform particles and smaller size.
[0028] 2) The pretreated biogas residue is mixed with an aqueous solution of an activator, and after immersion, the mixture is filtered and dried to obtain modified biogas residue.
[0029] In some embodiments of the present invention, the activator may include at least one of KOH, ZnCl2, MgCl2, CaCl2 and FeCl3. In some embodiments of the present invention, the activator may be KOH, ZnCl2, MgCl2, CaCl2 or FeCl3. In other embodiments of the present invention, the activator may include two or more of KOH, ZnCl2, MgCl2, CaCl2 and FeCl3. The above activators may improve the acidity and alkalinity of the matrix and / or the site activity, etc., which is beneficial to the subsequent loading of the catalyst active material, thereby facilitating the improvement of the catalyst activity.
[0030] In some embodiments of the present invention, in step 2), the mass ratio of pretreated biogas residue to activator can be 1:1-1:2.5. For example, the mass ratio of pretreated biogas residue to activator can be 1:1, 1:1.5, 1:2, 1:2.5, etc. Thus, the pretreated biogas residue and the activator have a suitable mass ratio, which is beneficial to sufficient contact and reaction between the activator and the pretreated biogas residue, thereby helping to improve the acidity and alkalinity of the matrix and / or site activity, and further helping to improve the catalytic efficiency of the catalyst.
[0031] In the present invention, the concentration of the aqueous solution of the activator is not specifically limited, and those skilled in the art can set and adjust the concentration of the aqueous solution of the activator according to actual needs.
[0032] In some embodiments of the present invention, the immersion time in step 2) may be 24-48 hours, for example, the immersion time may be 24 hours, 30 hours, 36 hours, 40 hours, 48 hours, etc. The immersion of the pretreated biogas residue and the aqueous solution of the activator for a long time is conducive to the full contact and reaction between the activator and the biogas residue, thereby modifying the biogas residue and making it have suitable acidity and alkalinity and higher site activity.
[0033] 3) Pyrolyzing the modified biogas residue obtained in step 2) at a temperature of 500°C-800°C in a N2 atmosphere to obtain a biogas residue biochar matrix.
[0034] In some embodiments of the present invention, the modified biogas residue prepared in step 2) may be pyrolyzed at 500°C, 600°C, 650°C, 700°C, 750°C or 800°C to decompose the biogas residue to form biochar.
[0035] In some embodiments of the present invention, during the pyrolysis process, the flow rate of N2 can be 20ml / min-40ml / min. For example, the flow rate of N2 can be 20ml / min, 25ml / min, 30ml / min, 35ml / min or 40ml / min. Continuously introducing N2 with the above flow rate during the pyrolysis process is beneficial to removing water and impurities produced by the pyrolysis of sludge.
[0036] In some embodiments of the present invention, in step 3), the pyrolysis time can be 1-3 hours, for example, the pyrolysis time can be 1 hour, 1.5 hours, 2 hours, 2.5 hours or 3 hours, thereby, the biogas residue can be more fully pyrolyzed to remove organic matter in the biogas residue and obtain a biochar matrix with better performance.
[0037] 4) dissolving the biochar matrix of sludge in anhydrous ethanol to form a colloidal solution, magnetically stirring the colloidal solution at a temperature of 30° C.-60° C., adding an alcohol solution of a metal salt dropwise for impregnation during the stirring process, and continuing to stir until the solvent is completely evaporated to obtain a catalyst powder.
[0038] In some embodiments of the present invention, the colloidal solution may be magnetically stirred at 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C. Stirring at this temperature is beneficial to the volatilization of the organic solvent.
[0039] In some embodiments of the present invention, in step 4), the speed of magnetic stirring can be 400r / min-800r / min, for example, the speed of magnetic stirring can be 400r / min, 500r / min, 600r / min, 700r / min, 800r / min, etc. Stirring at the above speed is conducive to sufficient mixing of the colloidal solution and the alcohol solution of the metal salt, and is conducive to the volatilization of the organic solvent to obtain a mixture with uniform components.
[0040] In some embodiments of the present invention, the metal salt may include at least one of Ni nitrate, Fe nitrate, Co nitrate, Rh nitrate and Pd nitrate. The above metal salts can form metal catalysts after calcination and are loaded on the biochar matrix.
[0041] In some embodiments of the present invention, the metal salt may include two of Ni nitrate, Fe nitrate, Co nitrate, Rh nitrate and Pd nitrate, and the molar ratio of the two metal elements in the alcohol solution of the metal salt may be 1:3-3:1. In some embodiments of the present invention, the metal salt may include Ni nitrate and Fe nitrate, and the molar ratio of the nickel element to the iron element in the alcohol solution of the metal salt may be 1:3, 1:1, 2:1 or 3:1. In other embodiments of the present invention, the metal salt may include Ni nitrate and Co nitrate, or the metal salt may include Rh nitrate and Pd nitrate, or the metal salt may include Fe nitrate and Co nitrate.
[0042] In some embodiments of the present invention, in step 4), the mass of the metal element in the alcohol solution of the added metal salt is a, the mass of the biogas residue biochar matrix in the colloidal solution is b, and the value of a / (a+b) is 5%-20%. For example, the value of a / (a+b) can be 5%, 8%, 10%, 12%, 15% or 20%. The catalyst obtained after calcination of the raw materials in the above ratio has a suitable content of metal active substances, which is conducive to improving the catalytic efficiency of the catalyst.
[0043] In some embodiments of the present invention, in the alcohol solution of the metal salt, the solvent may include at least one of ethanol, n-propanol, isopropanol, n-butanol and isobutanol. In some specific embodiments of the present invention, in the alcohol solution of the metal salt, the solvent may be ethanol, n-propanol, isopropanol, n-butanol or isobutanol. In other specific embodiments of the present invention, in the alcohol solution of the metal salt, the solvent may be composed of two or more of ethanol, n-propanol, isopropanol, n-butanol and isobutanol.
[0044] 5) Calcine the catalyst powder at a temperature of 700° C. to 900° C. in a N 2 atmosphere, and then use a tablet press to press the calcined powder into tablets, crush it, and screen it to obtain a biogas dry reforming carbon-based catalyst.
[0045] In some embodiments of the present invention, the catalyst powder may be calcined at 700° C., 750° C., 800° C., 850° C. or 900° C. Thus, the metal salt may be decomposed to form a metal catalyst and loaded on the biochar matrix to obtain a catalyst with good stability.
[0046] In some embodiments of the present invention, in step 5), the calcination time may be 3-6 hours, for example, 3 hours, 4 hours, 5 hours or 6 hours, thereby facilitating the full reaction of the catalyst precursor and allowing the metal salt to completely react to generate a metal catalyst.
[0047] In some embodiments of the present invention, the particle size of the biogas dry reforming carbon-based catalyst may be 20 mesh-100 mesh, for example, the particle size of the biogas dry reforming carbon-based catalyst may be 20 mesh, 30 mesh, 50 mesh or 100 mesh. In some embodiments of the present invention, in step 5), a 20 mesh-100 mesh sieve may be used to sieve the crushed powder to obtain a catalyst with a suitable particle size and uniform particle size.
[0048] In general, the method proposed in the present invention for preparing biogas dry reforming catalyst has the following advantages:
[0049] 1. Preparing biochar from sludge, a by-product of anaerobic fermentation of kitchen waste, and using it as a matrix to synthesize carbon-based catalysts can provide a new way to solve the problem of anaerobic sludge disposal and the high-value utilization of sludge.
[0050] 2. The catalyst produced by the method proposed in the present invention has strong catalytic activity and good stability, and is suitable for biogas dry reforming technology.
[0051] 3. Biochar prepared using biogas residue as raw material is cheaper than commercial substrates, which can reduce the synthesis cost of biogas dry reforming catalysts, facilitate the large-scale application of biogas dry reforming technology, and realize the simultaneous resource utilization of biogas residue and biogas from anaerobic fermentation of kitchen waste.
[0052] In another aspect of the present invention, the present invention provides a biogas dry reforming carbon-based catalyst. In some embodiments of the present invention, the biogas dry reforming carbon-based catalyst is prepared using the method described above. As a result, the catalyst has good stability and strong catalytic activity, and is suitable for biogas dry reforming; the raw material source is wide, the matrix preparation cost is low, and it is conducive to reducing the synthesis cost of the catalyst.
[0053] In another aspect of the present invention, the present invention proposes the use of the above-mentioned biogas dry reforming carbon-based catalyst in biogas dry reforming. The biogas dry reforming carbon-based catalyst has good stability and strong catalytic activity, can simultaneously convert CH4 and CO2 into synthesis gas, and promote the high added value conversion of biogas to downstream chemical gas production.
[0054] The present invention will be described below by specific examples, and it will be appreciated by those skilled in the art that the following specific examples are only for illustrative purposes, and do not limit the scope of the present invention in any way. In addition, in the following examples, unless otherwise specified, the materials and equipment used are all commercially available. If in the following examples, specific processing conditions and processing methods are not clearly described, then conditions and methods known in the art can be used to process.
[0055] Example 1
[0056] Reference Figure 1 A method for preparing a biogas dry reforming carbon-based catalyst by pyrolyzing biochar from biogas residue comprises the following steps:
[0057] 1) drying the anaerobic digestate from kitchen waste at 80° C. for 12 hours, crushing it with a plant crusher after drying, and sieving it with a 40-mesh sieve to obtain pretreated digestate;
[0058] 2) mixing the pretreated biogas residue obtained in step 1) with an aqueous solution of an activator ZnCl2, wherein the mass ratio of the pretreated biogas residue to ZnCl2 is 1:1, and after immersion for 24 hours, filtering and drying to obtain modified biogas residue;
[0059] 3) pyrolyzing the modified biogas residue obtained in step 2) at 600° C. in a N2 atmosphere for 1 hour to obtain a biochar matrix;
[0060] 4) Dissolve 1.1151 g of Ni(NO3)2·6H2O solid and 1.6233 g of Fe(NO3)3·9H2O solid in 40 ml of anhydrous ethanol to obtain an active metal salt alcohol solution;
[0061] Dissolve 4.05 g of the biochar matrix obtained in step 3) in 50 ml of anhydrous ethanol to form a uniform colloidal solution;
[0062] The colloidal solution was magnetically stirred at 60°C and 600 r / min, and the active metal salt alcohol solution was added dropwise for impregnation, and the stirring was continued until the ethanol was completely volatilized to obtain a catalyst powder;
[0063] 5) placing the catalyst powder obtained in step 4) in a tubular furnace and calcining it at 700°C in a N2 atmosphere for 6 hours; using a tablet press to press the calcined powder into tablets, crush it, and sieve it to obtain catalyst product particles of 20-100 mesh.
[0064] Example 2
[0065] Reference Figure 1 A method for preparing a biogas dry reforming carbon-based catalyst by pyrolyzing biochar from biogas residue comprises the following steps:
[0066] 1) drying the anaerobic digestate from kitchen waste at 80° C. for 12 hours, crushing it with a plant crusher after drying, and sieving it with a 40-mesh sieve to obtain pretreated digestate;
[0067] 2) mixing the pretreated biogas residue obtained in step 1) with an aqueous solution of an activator FeCl3, wherein the mass ratio of the pretreated biogas residue to FeCl3 is 1:1, and after immersion for 24 hours, filtering and drying to obtain modified biogas residue;
[0068] 3) pyrolyzing the modified biogas residue obtained in step 2) at 600° C. in a N2 atmosphere for 1 hour to obtain a biochar matrix;
[0069] 4) Dissolve 1.1151 g of Ni(NO3)2·6H2O solid and 1.6644 g of Co(NO3)2·6H2O solid in 40 ml of anhydrous ethanol to obtain an active metal salt alcohol solution;
[0070] Dissolve 4.05 g of the biochar matrix obtained in step 3) in 50 ml of anhydrous ethanol to form a uniform colloidal solution;
[0071] The colloidal solution was magnetically stirred at a temperature of 50°C and a speed of 600 r / min, and the active metal salt alcohol solution was added dropwise for impregnation, and the stirring was continued until the ethanol was completely volatilized to obtain a catalyst powder;
[0072] 5) placing the catalyst powder obtained in step 4) in a tubular furnace and calcining it at 700°C in a N2 atmosphere for 8 hours; using a tablet press to press the calcined powder into tablets, crush it, and sieve it to obtain catalyst product particles of 20-100 mesh.
[0073] Example 3
[0074] The difference from Example 1 is that the active agent in step 2) is CaCl2, and the other steps and parameters are the same as those in Example 1.
[0075] Example 4
[0076] The difference from Example 1 is that the immersion time in step 2) is 48 hours, and the other steps and parameters are the same as those in Example 1.
[0077] Example 5
[0078] The difference from Example 1 is that in step 2), the mass ratio of pretreated biogas slag to activator ZnCl2 is 1:1.5, and the other steps and parameters are the same as those in Example 1.
[0079] Example 6
[0080] The difference from Example 2 is that the pyrolysis temperature in step 3) is 700°C, and the other steps and parameters are the same as those in Example 2.
[0081] The specific surface areas and reforming conversion rates of the carbon-based catalyst products prepared in Examples 1 to 6 are shown in Table 1.
[0082] Table 1
[0083]
[0084] It can be seen from Table 1 that the specific surface area of the biogas residue dry reforming carbon-based catalyst prepared by the method of the present invention can reach tens to hundreds of m 2 / g, suitable for use as a catalyst; the biogas reforming test results show that the catalyst proposed in the present invention has good catalytic activity and stability.
[0085] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine different embodiments or examples described in this specification and the features of different embodiments or examples without contradiction.
[0086] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a biogas dry reforming carbon-based catalyst by pyrolyzing biochar from biogas residue, characterized in that: The following steps are involved: 1) drying the anaerobic digestate from kitchen waste, crushing and screening the dried digestate to obtain pretreated digestate; 2) mixing the pretreated biogas residue with an aqueous solution of an activator, immersing, filtering and drying the pretreated biogas residue to obtain modified biogas residue; 3) pyrolyzing the modified biogas residue obtained in step 2) at a temperature of 500° C. to 800° C. in a N2 atmosphere to obtain a biogas residue biochar matrix; 4) dissolving the biogas residue biochar matrix in anhydrous ethanol to form a colloidal solution, subjecting the colloidal solution to magnetic stirring at a temperature of 30° C. to 60° C., adding a metal salt alcohol solution dropwise during stirring for impregnation, and continuing stirring until the solvent is completely volatilized to obtain a catalyst powder; 5) calcining the catalyst powder at a temperature of 700° C. to 900° C. in a N 2 atmosphere, and then using a tablet press to press the calcined powder into tablets, crush it, and screen it to obtain a biogas dry reforming carbon-based catalyst.
2. The method according to claim 1, characterized in that In step 4), the mass of the metal element in the alcohol solution of the added metal salt is a, the mass of the biogas residue biochar matrix in the colloidal solution is b, and the value of a / (a+b) is 5%-20%.
3. The method according to claim 1, characterized in that The metal salt includes at least one of Ni nitrate, Fe nitrate, Co nitrate, Rh nitrate and Pd nitrate; And / or, in the alcohol solution of the metal salt, the solvent includes at least one of ethanol, n-propanol, isopropanol, n-butanol and isobutanol.
4. The method according to claim 1, characterized in that: The metal salt comprises two of Ni nitrate, Fe nitrate, Co nitrate, Rh nitrate and Pd nitrate. In the alcohol solution of the metal salt, the molar ratio of the two metal elements is 1:3-3:
1.
5. The method according to claim 1, characterized in that The activator includes at least one of KOH, ZnCl2, MgCl2, CaCl2 and FeCl3.
6. The method according to any one of claims 1 to 5, characterized in that In step 1), the anaerobic digestate of kitchen waste is dried at 80°C-95°C for 12-24 hours; And / or, in step 1), sieving is performed using a 20-100 mesh sieve.
7. The method according to any one of claims 1 to 5, characterized in that In step 2), the mass ratio of the pretreated biogas residue to the activator is 1:1-1:2.5; And / or, the immersion time in step 2) is 24-48 hours.
8. The method according to any one of claims 1 to 5, characterized in that At least one of the following conditions is met: In step 3), the pyrolysis time is 1-3 hours; In step 4), the speed of magnetic stirring is 400r / min-800r / min; In step 5), the calcination time is 3-6 hours; The particle size of the biogas dry reforming carbon-based catalyst is 20 meshes to 100 meshes.
9. A biogas dry reforming carbon-based catalyst, characterized in that: The biogas dry reforming carbon-based catalyst is prepared by the method described in any one of claims 1-8.
10. Use of the biogas dry reforming carbon-based catalyst according to claim 9 in biogas dry reforming.
Citation Information
Patent Citations
Method for preparing heterogeneous Fenton catalyst from waste biogas residues and application
CN106040241A
Preparation method of ultrathin flexible carbon nanosheet oxygen reduction catalyst based on anaerobic fermentation biogas residues
CN111129523A
Preparation method and application of high-activity catalyst for hydrogen production through reforming of methane and carbon dioxide
CN113522322A
Method for removing carbon dioxide by in-situ utilization of biogas residue as biogas purification
CN115739022A
Method for preparing biochar and hydrogen by utilizing anaerobic fermentation byproducts