Catalyst for preparing olefin through hydrogenation of carbon dioxide as well as preparation method and application of catalyst
Through the preparation method of Fe-Cu-Ce catalyst, the problem of low selectivity and conversion rate of low carbon olefin catalysts under normal pressure is solved, and high-efficiency preparation of low carbon olefins is achieved, reducing industrial costs and energy consumption .
Patent Information
- Application Number
- CN202410904131.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-01
AI Technical Summary
The existing carbon dioxide hydrogenation catalysts for preparing low-carbon olefins have poor selectivity and low CO2 conversion at normal pressure, resulting in high industrial application costs and increased energy consumption.
By using the preparation method of Fe-Cu-Ce catalyst, by mixing the metal salt solution with an alkaline solution, adjusting the pH to completely precipitate the metal, and roasting it in a hydrogen/inert gas mixture to form a mixed valence metal oxide, so as to Improve the activity and selectivity of the catalyst.
The total selectivity of low-carbon olefins is greater than 30% and the CO2 conversion rate exceeds 10% under normal pressure, which reduces industrial manufacturing costs, and is easy to produce and recycle the catalyst, which has good environmental friendliness.
Smart Images

Figure BDA0004931467080000091 
Figure BDA0004931467080000101 
Figure BDA0004931467080000102
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of catalysts, and more specifically, relates to a catalyst for preparing olefins by hydrogenating carbon dioxide, and a preparation method and application thereof. Background Art
[0002] With energy and environmental issues becoming increasingly prominent and global energy demand continuing to grow, it is crucial to develop sustainable, low-carbon chemical synthesis methods. Olefins are important organic compounds that are widely used in chemical industries such as gasoline, plastics, and solvents. However, traditional olefin synthesis methods often rely on fossil fuel resources such as petroleum and natural gas, which not only has a negative impact on the environment, but also faces challenges in resource depletion and energy security. Carbon dioxide hydrogenation to olefins is a promising green synthesis route that not only reduces greenhouse gas emissions and improves environmental and ecological issues, but also realizes the resource utilization of carbon dioxide and promotes the green and low-carbon transformation of the energy structure.
[0003] The principles of CO2 hydrogenation to olefins can be mainly divided into two categories: methanol intermediate pathway and CO intermediate pathway. For the methanol intermediate pathway, according to Le Chatelier's principle, high pressure is conducive to the forward reaction of CO2 to methanol in the first step, but is not conducive to the forward reaction of methanol to olefins (MTO) in the second step. Therefore, there is a trade-off between the first and second steps of the methanol intermediate pathway, which poses a major challenge to the design of the catalytic system. For the CO intermediate pathway, the first step is the reverse water gas reaction (RWGS), where CO2 is first reduced to CO through RWGS, and then the generated CO is activated to form CHx (x<3) species. Then, the CHx species undergoes CC coupling through Fischer-Tropsch synthesis (FTS) to form CnHm (n≥2) intermediates. This method is currently the commonly used pathway for CO2 hydrogenation to olefins. Iron-based materials have been proven to be suitable candidates for CO2 hydrogenation to produce light olefins.
[0004] For example, Chinese patent application CN 117563605 A provides a method for preparing low-carbon olefins by hydrogenation of carbon dioxide with a non-precious metal catalyst, but the catalyst prepared by the method is applied in the hydrogenation of carbon dioxide, and the selectivity of low-carbon olefins is limited. In addition, the catalyst for producing olefins by hydrogenation of carbon dioxide still requires high temperature and high pressure during the hydrogenation reaction, which greatly increases the cost and energy consumption of industrial equipment. Therefore, the technology still faces some challenges in industrial applications. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the existing catalyst for preparing light olefins by hydrogenation of carbon dioxide at normal pressure, such as poor selectivity for preparing light olefins by hydrogenation and poor CO2 conversion rate, and to provide a method for preparing the catalyst.
[0006] The object of the present invention is to provide a catalyst.
[0007] Another object of the present invention is to provide the use of the catalyst of the present invention in the preparation of light olefins by hydrogenation of carbon dioxide.
[0008] Another object of the present invention is to provide a method for preparing light olefins by hydrogenating carbon dioxide.
[0009] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0010] A method for preparing a catalyst comprises the following steps:
[0011] The metal salt solution and the alkaline solution are mixed, the pH is adjusted so that the metal in the metal salt solution is completely precipitated, and then the solution with the precipitate is crystallized; the crystallized precipitate is calcined in a hydrogen / inert gas mixture at 300-600° C. to obtain a catalyst;
[0012] The metals in the metal salt solution include Fe, Cu and Ce in a molar ratio of 1.5 to 2.5:1:1.5 to 2.5;
[0013] The metal ions in the alkaline solution are sodium ions or potassium ions.
[0014] Cu is a mild hydrogenation catalyst, which can inhibit the excessive hydrogenation of products to produce alkanes in the reaction of carbon dioxide hydrogenation to olefins; iron-based active phase is the best choice for olefin production, so the present invention proposes a preparation method of Fe-Cu-Ce catalyst. X The reaction of RWGS and FTS is promoted, and the metal oxide of Ce is formed by the introduction of Ce, which provides a large number of Ce-O bonds and thus a large number of oxygen vacancies, thereby improving the carbon dioxide conversion rate of the Fe-based catalyst. The formation of Cu metal and its oxide promotes the RWGS reaction while suppressing the excessive hydrogenation of olefins to alkanes by the Fe-based catalyst. However, when too much Cu element is introduced, the Fe catalyst will be more conducive to the RWGS reaction rather than the FTS synthesis to prepare olefins. When the Ce content is too much, the by-product CH4 content will increase significantly, thereby reducing the selectivity of olefins. Therefore, only when the molar ratio of the metal is within the range described in the present invention can it have a good promoting catalytic activity.
[0015] The present invention adjusts the pH to completely precipitate the metal, and then further crystallizes the solution with the precipitate, so that the precipitate therein becomes an oxide, which is more conducive to the subsequent catalytic performance.
[0016] The calcination of the present invention is mainly to obtain a mixed-valence metal oxide. The performance and morphology of the catalyst are greatly affected by the calcination temperature. Too high or too low calcination temperature will lead to reduced catalytic performance. Too high calcination temperature will lead to catalyst morphology aggregation, larger crystal particle size, smaller surface area, and thus reduced catalyst activity; too low calcination temperature will lead to incomplete formation of catalyst crystal particles, fewer metal active centers, and reduced catalytic activity. At the same time, high catalytic activity can be attributed to the interaction of metal precursors of Fe, Cu and Ce under high temperature calcination to form highly dispersed or aggregated multi-metal binding sites.
[0017] Furthermore, the alkali in the alkaline solution is one or more of sodium hydroxide, sodium acetate and potassium hydroxide.
[0018] The solvent of the alkaline solution is water.
[0019] Furthermore, the crystallization temperature is 150-240°C; preferably, the crystallization temperature is 160-200°C.
[0020] Furthermore, the crystallization time is 12 to 36 hours; preferably, the crystallization time is 20 to 30 hours.
[0021] Furthermore, in the hydrogen / inert gas mixture, the volume ratio of hydrogen to inert gas is 1:8-10; preferably, in the hydrogen / inert gas mixture, the volume ratio of hydrogen to inert gas is 1:9.
[0022] Furthermore, the inert gas is one or both of nitrogen and argon.
[0023] Furthermore, the adjusted pH is ≥ 9; preferably, the adjusted pH is 9-11.
[0024] Furthermore, the calcination time is 1 to 4 hours; preferably, the calcination time is 1.5 to 3 hours; more preferably, the calcination time is 2 hours.
[0025] Preferably, the calcination temperature is 300-500°C; more preferably, the calcination temperature is 350-450°C.
[0026] The present invention protects the catalyst prepared by the preparation method.
[0027] At the same time, the present invention also protects the use of the catalyst in preparing light olefins by hydrogenating carbon dioxide.
[0028] The catalyst prepared by the present invention is used for the carbon dioxide hydrogenation reaction, and the reaction is carried out under normal pressure (0.1 MPa). The total selectivity of the finally prepared low-carbon olefins is greater than 30%, and the carbon dioxide conversion rate is greater than 10%.
[0029] More specifically, the low-carbon olefin is an olefin having 2 to 4 carbon atoms, such as ethylene, propylene, butene and the like.
[0030] The present invention provides a method for preparing low-carbon olefins by hydrogenating carbon dioxide. A mixed gas of H2 and CO2 is introduced into the catalyst of the present invention to carry out a hydrogenation reaction at 280-300°C and 0.1-4MPa.
[0031] Furthermore, in the mixed gas of H2 and CO2, the volume ratio of H2:CO2 is 3 to 1:1; preferably, the volume ratio of H2:CO2 is 3:1.
[0032] Furthermore, the space velocity is 2000 to 12000 mL / h·g cat Within this space velocity range, the use of the catalyst of the present invention in the hydrogenation of carbon dioxide to prepare light olefins can ultimately obtain a higher light olefin yield and a better carbon dioxide conversion rate.
[0033] Preferably, the space velocity is 2400 to 12000 mL / h·g cat .
[0034] In the test example of the present invention, at 1 bar (0.1 MPa, normal pressure), when the air velocity is 2400 mL / h·g cat When the space velocity is 12000mL / h·g cat When the volume ratio of H2:CO2 is 3:1, the catalyst of the present invention is used to carry out the hydrogenation of carbon dioxide to olefins, and the final total selectivity of light olefins is as high as 48.77%, and the CO2 conversion rate is 10.27%. When the volume ratio of H2:CO2 is further increased to 4:1, the final total selectivity of light olefins is only 25.83%.
[0035] The present invention has the following beneficial effects:
[0036] (1) The present invention uses a simple metal co-precipitation treatment process and crystallization reaction, followed by calcination to obtain a metal catalyst. The catalyst raw material in the present invention is cheap and the preparation method is simple, which is easy to scale up for industrial application;
[0037] (2) The catalyst of the present invention does not contain sulfur and no organic matter is added during the preparation process to cause environmental pollution, thereby reducing environmental pollution and harm to human body;
[0038] (3) The catalyst prepared by the present invention can catalyze the carbon dioxide hydrogenation reaction under the reaction conditions of 300°C and 1 bar (0.1 MPa), that is, under low temperature and normal pressure conditions, and the total selectivity of the low-carbon olefins finally prepared is greater than 30%, and the carbon dioxide conversion rate is more than 10%, which can greatly reduce the industrial manufacturing cost and is conducive to industrial production. The technical effect is significantly better than the existing carbon dioxide hydrogenation catalyst (all of which need to be under a pressurized environment to have a good effect);
[0039] (4) The catalyst of the present invention has high selectivity and convenient recyclability. The multi-metal synergistic effect can reduce the activation energy and improve the catalytic activity. It has broad application prospects in the fields of catalytic hydrogenation, oxidation, electrochemistry, etc. DETAILED DESCRIPTION
[0040] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0041] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0042] Example 1 A catalyst for hydrogenating carbon dioxide to olefins
[0043] The preparation method of the catalyst for hydrogenating carbon dioxide to olefins described in this embodiment comprises the following steps:
[0044] Weigh 8.0798 g of ferric nitrate (Fe(NO3)3·9H2O), 2.4165 g of copper nitrate (Cu(NO3)2·3H2O), and 8.6844 g of cerium nitrate (Ce(NO3)3·6H2O) and dissolve them in 60 mL of deionized water to obtain a metal salt mixture (molar ratio of Fe:Cu:Ce=2:1:2) and stir until transparent. Then prepare 5M NaOH alkaline solution is added dropwise to the metal salt solution at a speed of 60 rpm through a peristaltic pump, and stirred continuously until the pH is 10, so that the metal ions in the solution are completely precipitated, and then the solution with the precipitate is transferred to a crystallization kettle and kept at 180°C for 24 hours for crystallization. The crystallized precipitate is then centrifuged at 70,000 rpm for 5 minutes, washed with deionized water, and then dried at 80°C in an oven, and then calcined at 400°C for 2 hours in a mixed gas of nitrogen and hydrogen (nitrogen: hydrogen is 9:1), and finally a catalyst for hydrogenation of carbon dioxide to olefins is obtained, which is marked as Fe-Cu-Ce-Na-10.
[0045] Example 2 A catalyst for hydrogenating carbon dioxide to olefins
[0046] The difference between this embodiment and embodiment 1 is that a 5M KOH alkaline solution is prepared, and the KOH alkaline solution is added dropwise to the metal salt solution at a speed of 60 rpm by a peristaltic pump, and stirred continuously until the pH reaches 10. The other conditions are the same, and the prepared catalyst for hydrogenation of carbon dioxide to olefins is marked as Fe-Cu-Ce-K-10.
[0047] Example 3 A catalyst for hydrogenating carbon dioxide to olefins
[0048] The difference between this embodiment and embodiment 1 is that the catalyst for hydrogenation of carbon dioxide to olefins is finally obtained by calcining at 300° C. for 4 h in a mixture of nitrogen and hydrogen (nitrogen:hydrogen is 9:1) while other conditions are the same.
[0049] Comparative Example 1 A catalyst for hydrogenating carbon dioxide to olefins
[0050] The difference between this comparative example and Example 1 is that the amount of copper nitrate (Cu(NO3)2·6H2O) added is 4.8312 g, cerium nitrate is not added, and the other experimental steps are the same.
[0051] The prepared catalyst for hydrogenation of carbon dioxide to olefins is marked as Fe-Cu-Na-10.
[0052] Comparative Example 2 A catalyst for hydrogenating carbon dioxide to olefins
[0053] The difference between this comparative example and Example 1 is that copper nitrate is not added, and the other experimental steps are the same.
[0054] The prepared catalyst for hydrogenating carbon dioxide to olefins is marked as Fe-Ce-Na-10.
[0055] Comparative Example 3 A catalyst for hydrogenating carbon dioxide to olefins
[0056] The difference between this comparative example and Example 1 is that no ferric nitrate is added, and the other experimental steps are the same.
[0057] The prepared catalyst for hydrogenation of carbon dioxide to olefins is marked as Cu-Ce-Na-10.
[0058] Comparative Example 4 A catalyst for hydrogenating carbon dioxide to olefins
[0059] The difference between this comparative example and Example 1 is that 4.0410 g of ferric nitrate (Fe(NO3)3·9H2O), 2.4165 g of copper nitrate (Cu(NO3)2·3H2O), and 4.3422 g of cerium nitrate (Ce(NO3)3·6H2O) are weighed and dissolved in 60 mL of deionized water to obtain a metal salt mixture (molar ratio of Fe:Cu:Ce=1:1:1) and stirred until transparent, and then the other conditions are the same. The prepared catalyst for hydrogenation of carbon dioxide to olefins is marked as Fe-Cu-Ce-1-1-1-Na-10.
[0060] Comparative Example 5 A catalyst for hydrogenating carbon dioxide to olefins
[0061] The difference between this comparative example and Example 1 is that 4.0410 g of ferric nitrate (Fe(NO3)3·9H2O), 2.4165 g of copper nitrate (Cu(NO3)2·3H2O), and 8.6844 g of cerium nitrate (Ce(NO3)3·6H2O) are weighed and dissolved in 60 mL of deionized water to obtain a metal salt mixture (molar ratio of Fe:Cu:Ce=1:1:2) and stirred evenly until transparent, and then the other conditions are the same. The prepared catalyst for hydrogenation of carbon dioxide to olefins is marked as Fe-Cu-Ce-1-1-2-Na-10.
[0062] Comparative Example 6 A catalyst for hydrogenating carbon dioxide to olefins
[0063] The difference between this comparative example and Example 1 is that 4.0410 g of ferric nitrate (Fe(NO3)3·9H2O), 4.8312 g of copper nitrate (Cu(NO3)2·6H2O), and 8.6844 g of cerium nitrate (Ce(NO3)3·6H2O) are weighed and dissolved in 60 mL of deionized water to obtain a metal salt mixture (molar ratio of Fe:Cu:Ce=1:2:2) and stirred until transparent, and then the other conditions are the same. The prepared catalyst for hydrogenation of carbon dioxide to olefins is marked as Fe-Cu-Ce-1-2-2-Na-10.
[0064] Comparative Example 7 A catalyst for hydrogenating carbon dioxide to olefins
[0065] The difference between this comparative example and Example 1 is that 4.0410 g of ferric nitrate (Fe(NO3)3·9H2O), 4.8312 g of copper nitrate (Cu(NO3)2·6H2O) and 4.3422 g of cerium nitrate (Ce(NO3)3·6H2O) are weighed and dissolved in 60 mL of deionized water to obtain a metal salt mixture (molar ratio of Fe:Cu:Ce=1:2:1) and stirred until transparent. The remaining conditions are then the same, and the prepared catalyst for hydrogenation of carbon dioxide to olefins is marked as Fe-Cu-Ce-1-2-1-Na-10.
[0066] Comparative Example 8 A catalyst for hydrogenating carbon dioxide to olefins
[0067] The difference between this comparative example and Example 1 is that 8.0798 g of ferric nitrate (Fe(NO3)3·9H2O), 2.4165 g of copper nitrate (Cu(NO3)2·3H2O), and 4.3422 g of cerium nitrate (Ce(NO3)3·6H2O) are weighed and dissolved in 60 mL of deionized water to obtain a metal salt mixture (molar ratio of Fe:Cu:Ce=2:1:1) and stirred until transparent, and then the other conditions are the same. The prepared catalyst for hydrogenation of carbon dioxide to olefins is marked as Fe-Cu-Ce-2-1-1-Na-10.
[0068] Comparative Example 9 A catalyst for hydrogenating carbon dioxide to olefins
[0069] The difference between this comparative example and Example 1 is that 8.0798 g of ferric nitrate (Fe(NO3)3·9H2O), 4.8312 g of copper nitrate (Cu(NO3)2·6H2O), and 4.3422 g of cerium nitrate (Ce(NO3)3·6H2O) are weighed and dissolved in 60 mL of deionized water to obtain a metal salt mixture (molar ratio of Fe:Cu:Ce=2:1:2) and stirred until transparent, and then the other conditions are the same. The prepared catalyst for hydrogenation of carbon dioxide to olefins is marked as Fe-Cu-Ce-2-2-1-Na-10.
[0070] Comparative Example 10 A catalyst for hydrogenating carbon dioxide to olefins
[0071] The difference between this comparative example and Example 1 is that a 5M NH3·H2O alkaline solution is prepared, and the NH3·H2O alkaline solution is added dropwise to the metal salt solution at a speed of 60 rpm by a peristaltic pump, and continuously stirred until the pH reaches 10. Then the other conditions are the same, and the prepared catalyst for hydrogenation of carbon dioxide to olefins at normal pressure is marked as Fe-Cu-Ce-NH3-10.
[0072] In this comparative example, the NaOH alkaline solution in Example 1 is replaced by NH3·H2O alkaline solution.
[0073] Comparative Example 11 A catalyst for hydrogenating carbon dioxide to olefins
[0074] The difference between this comparative example and Example 1 is that a 5M NaOH alkaline solution is prepared, and the NaOH alkaline solution is added dropwise to the metal salt solution at a speed of 60 rpm by a peristaltic pump, and continuously stirred until the pH reaches 8. Then the other conditions are the same, and the prepared catalyst for hydrogenation of carbon dioxide to olefins at normal pressure is marked as Fe-Cu-Ce-Na-8.
[0075] In this comparative example, the pH in Example 1 was adjusted to 8 instead of 10.
[0076] Comparative Example 12 A catalyst for hydrogenating carbon dioxide to olefins
[0077] The difference between this comparative example and comparative example 10 is that the mixture is continuously stirred until the pH value reaches 8, and the other conditions are the same. The prepared catalyst for hydrogenation of carbon dioxide to olefins under normal pressure is marked as Fe-Cu-Ce-NH3-8.
[0078] Comparative Example 13 A catalyst for hydrogenating carbon dioxide to olefins
[0079] The difference between this comparative example and comparative example 11 is that the NaOH alkaline solution in comparative example 11 is replaced by Na2CO3 alkaline solution, and the other conditions are the same. The prepared catalyst for hydrogenation of carbon dioxide to olefins at normal pressure is marked as Fe-Cu-Ce-Na2-8.
[0080] Comparative Example 14 A catalyst for hydrogenating carbon dioxide to olefins
[0081] The difference between this comparative example and Example 1 is that a 5M LiOH alkaline solution is prepared, and the LiOH alkaline solution is added dropwise to the metal salt solution at a speed of 60 rpm by a peristaltic pump, and stirred continuously until the pH reaches 10. Then the other conditions are the same, and the prepared metal catalyst for hydrogenation of carbon dioxide to olefins at normal pressure is marked as Fe-Cu-Ce-Li-10.
[0082] In this comparative example, the NaOH alkaline solution in Example 1 is replaced by a LiOH alkaline solution.
[0083] Comparative Example 15 A catalyst for hydrogenating carbon dioxide to olefins
[0084] Weigh 8.0798 g of ferric nitrate (Fe(NO3)3·9H2O), 2.4165 g of copper nitrate (Cu(NO3)2·3H2O), and 8.6844 g of cerium nitrate (Ce(NO3)3·6H2O) and dissolve them in 60 mL of deionized water to obtain a metal salt mixture (molar ratio of Fe:Cu:Ce=2:1:2) and stir until transparent. Then prepare a 5M NH3·H2O alkaline solution, and add the NH3·H2O alkaline solution dropwise to the metal salt solution at 60 rpm through a peristaltic pump, and stir continuously until the pH is 10, so that the metal ions in the solution are completely precipitated. Then transfer the solution with the precipitate to a crystallization kettle, keep it at 180°C for 24 hours for crystallization, and then centrifuge the obtained precipitate at 70,000 rpm for 5 min, wash it with deionized water, and then dry it in an oven at 80°C to obtain a catalyst precursor. Then weigh 2.3624 g of calcium nitrate (Ca(NO3)2·4H2O) and dissolve it in 2 mL of deionized water to prepare a 5M Ca(NO3)2 solution. The 5M Ca(NO3)2 solution is dropped onto the catalyst precursor by an equal volume impregnation method and impregnated overnight. Finally, it is dried at 80°C in an oven and calcined at 400°C in a mixture of nitrogen and hydrogen (nitrogen: hydrogen is 9:1) for 2 h. The prepared metal catalyst for hydrogenation of carbon dioxide to olefins at normal pressure is labeled Fe-Cu-Ce-NH3-Ca-10.
[0085] The difference compared with Comparative Example 10 is that after crystallization and drying, it is first impregnated with calcium nitrate and then dried and calcined. Comparative Example 16 A catalyst for hydrogenating carbon dioxide to olefins
[0086] The difference from Comparative Example 15 is that Ca(NO3)2 is replaced by Mg(NO3)2·6H2O, and the other conditions are the same. The prepared catalyst for hydrogenation of carbon dioxide to olefins at normal pressure is marked as Fe-Cu-Ce-NH3-Mg-10.
[0087] Comparative Example 17 A catalyst for hydrogenating carbon dioxide to olefins
[0088] The difference from Comparative Example 15 is that Ca(NO3)2 is replaced by KNO3, and the other conditions are the same. The prepared catalyst for hydrogenation of carbon dioxide to olefins at normal pressure is marked as Fe-Cu-Ce-NH3-K-10.
[0089] Comparative Example 18 A catalyst for hydrogenating carbon dioxide to olefins
[0090] The difference from Comparative Example 15 is that Ca(NO3)2 is replaced by NaNO3, and the other conditions are the same. The prepared catalyst for hydrogenation of carbon dioxide to olefins at normal pressure is marked as Fe-Cu-Ce-NH3-Na-10.
[0091] Comparative Example 19 A catalyst for hydrogenating carbon dioxide to olefins
[0092] The difference from Comparative Example 15 is that Ca(NO3)2 is replaced by LiNO3, and the other conditions are the same. The prepared catalyst for hydrogenation of carbon dioxide to olefins at normal pressure is marked as Fe-Cu-Ce-NH3-Li-10.
[0093] Test Example 1
[0094] In the test examples of the present invention, 0.25 g of the catalysts of Examples 1 to 2 and Comparative Examples 1 to 19 were weighed respectively, and confined in the middle of the fixed bed reactor with quartz sand. Then, a mixed gas of H2 and CO2 (total gas flow rate of 50 mL / min) was introduced, and the reaction was carried out at 300°C and 1 bar (0.1 MPa) for 6 hours. By volume ratio, H2:CO2=3:1. During the reaction, the product composition was analyzed online by gas chromatography at regular intervals.
[0095] Experimental results:
[0096] Catalyst raw material screening: The performance effects of the catalysts prepared in Example 1 and Comparative Examples 1 to 3 are shown in Table 1. It can be seen from Table 1 that the catalysts of Comparative Examples 2 and 3 can hardly produce light olefins by hydrogenation under normal pressure. Although the catalyst prepared in Comparative Example 1 can produce light olefins, its carbon dioxide conversion rate is only 7.72%. The catalyst prepared in Example 1 of the present invention has a carbon dioxide conversion rate of up to 10.27%. At the same time, the total selectivity of light olefins is as high as 43.77% (an increase of 40.42% compared with Comparative Example 3), and the catalyst has the best performance effect.
[0097] Table 1 Performance effect of the catalysts prepared in Example 1 and Comparative Examples 1 to 3
[0098]
[0099] Note: C3-C4 o Alkane products with 3 to 4 carbon atoms; C3-C4 = The product is an olefin product with 3 to 4 carbon atoms; the total selectivity of low-carbon olefins is C2H4, C3-C4 = The sum of the percentages of the contents.
[0100] Screening of catalyst raw material composition ratio: Table 2 is a table of catalyst performance effects of Examples 4 to 9 and Example 1. We prepared catalysts with different molar ratios of Fe, Cu, and Ce, including 7 different ratios, to adjust the Fe content alone, the Cu content alone, the Ce content alone, the Fe and Ce contents, the Fe and Cu contents, the Cu and Ce contents, and other catalysts with different content characteristics. According to the results in Table 2, when the Fe and Ce contents increased and the Cu content remained unchanged, that is, the molar ratio Fe:Cu:Ce=2:1:2 (Example 1), the catalyst performance was the best, the total selectivity of light olefins was as high as 48.77%, and the carbon dioxide conversion rate was 10.27%.
[0101] Table 2 Catalyst performance results of comparative examples 4 to 9 and embodiment 1
[0102]
[0103] Note: C3-C4 o Alkane products with 3 to 4 carbon atoms; C3-C4 = The product is an olefin product with 3 to 4 carbon atoms; the total selectivity of low-carbon olefins is C2H4, C3-C4 = The sum of the percentages of the contents.
[0104] Catalyst alkaline solution and pH screening: The present invention selects different alkaline solutions NaOH, NH3·H2O, Na2CO3, KOH, LiOH and the like as alkaline precipitants and adjusts pH=8 and pH=10 to prepare catalysts, and explores the influence of different alkaline precipitants and pH. As shown in the results in Table 3, when NaOH and KOH are used as alkaline precipitants, the total selectivity of light olefins is significantly higher than that of NH3·H2O as the alkaline precipitant. Among the performances of the 13 catalysts (different alkaline agents), the best is to select NaOH and KOH as alkaline precipitants and adjust pH=10, and the total selectivity of light olefins is 43.77% and 31.01% respectively, and the carbon dioxide conversion rate is 10.27% and 17.29% respectively.
[0105] Table 3
[0106]
[0107]
[0108] Note: C3-C4 o Alkane products with 3 to 4 carbon atoms; C3-C4 = The product is an olefin product with 3 to 4 carbon atoms; the total selectivity of low-carbon olefins is C2H4, C3-C4 = The sum of the percentages of the contents.
[0109] Experimental Example 2 Effects of different space velocities, different H2 / CO2 ratios, and different temperatures on the catalytic performance of the catalyst in the carbon dioxide hydrogenation catalytic experiment
[0110] Effect of different space velocities on the catalytic performance of catalysts: 0.25 g of catalyst from Example 1 (space velocity 12000 mL / h·g cat )、0.625g(space velocity 4800mL / h·g cat )、1.25g(space velocity 2400mL / h·g cat )、1.5g(space velocity 2000mL / h·g cat ), which was confined in the middle of the fixed bed reactor with quartz sand, and then a mixed gas of H2 and CO2 was introduced (the total gas flow rate was 50 mL / min), and the reaction was carried out at 300°C and 1 bar for 6 hours. The volume ratio of H2:CO2 was 3:1. During the reaction, the product composition was analyzed online by gas chromatography at regular intervals.
[0111] The experimental results are shown in Table 4. The catalyst prepared in Example 1 of the present invention has a space velocity of 12000-2000 mL / h·g cat The total selectivity of low-carbon olefins is good at a space velocity of 2400 mL / h·g. As the space velocity decreases (the catalyst content increases), the total selectivity of olefins also increases. cat Under the conditions of , the total selectivity of light olefins in the experiment of catalyzing carbon dioxide hydrogenation with the catalyst of the present invention is the best, reaching 58.4%, and the carbon dioxide conversion rate is as high as 16.68%. However, if the space velocity is further reduced, the total selectivity of light olefins will decrease instead.
[0112] Table 4
[0113]
[0114] Note: C3-C4 o Alkane products with 3 to 4 carbon atoms; C3-C4 = The total selectivity of low-carbon olefins is C2H4, C3-C4 = The sum of the percentages of the contents.
[0115] Effect of different H2 / CO2 ratios on the catalytic performance of catalysts: Weigh 0.25 g of the catalyst of Example 1 and confine it in the middle of the fixed bed reactor with quartz sand. Then, a mixed gas of H2 and CO2 in different volume ratios is introduced (total gas flow rate is 50 mL / min), and the reaction is carried out at 300°C and 1 bar for 6 hours. During the reaction, the product composition is analyzed online by gas chromatography at regular intervals.
[0116] The experimental results are shown in Table 5. When the volume ratio of H2:CO2 is 3 to 1:1, the hydrogenation catalytic effect using the catalyst prepared in Example 1 of the present invention is better, among which the overall selectivity of light olefins is best when the volume ratio of H2:CO2 is 3:1.
[0117] Table 5
[0118]
[0119] Note: C3-C4 o Alkane products with 3 to 4 carbon atoms; C3-C4 = The total selectivity of low-carbon olefins is C2H4, C3-C4 = The sum of the percentages of the contents.
[0120] Effect of different temperatures on the catalytic performance of the catalyst: Weigh 0.25g of the catalyst of Example 1, confine it in the middle of the fixed bed reactor with quartz sand, then introduce a mixed gas of H2 and CO2 in different volume ratios, and react for 6 hours at 300℃, 320℃ or 350℃ at 1 bar (total gas flow rate of 50mL / min); during the reaction, the product composition is analyzed online by gas chromatography at regular intervals. It can be seen from the results in Table 6 that with the increase of temperature, the total selectivity of the catalyst for light olefins gradually decreases, and the optimal reaction temperature of the catalyst of the present invention is 300℃.
[0121] Table 6
[0122]
[0123]
[0124] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a catalyst, It is characterized in that The specific steps include: The metal salt solution and the alkaline solution are mixed, the pH is adjusted so that the metal in the metal salt solution is completely precipitated, and then the solution with the precipitate is crystallized; the crystallized precipitate is calcined in a hydrogen / inert gas mixture at 300-600° C. to obtain a catalyst; The metals in the metal salt solution include Fe, Cu and Ce in a molar ratio of 1.5 to 2.5:1:1.5 to 2.5; The metal ions in the alkaline solution are sodium ions or potassium ions.
2. The preparation method according to claim 1, It is characterized in that The alkali in the alkaline solution is one or more of sodium hydroxide, sodium acetate and potassium hydroxide.
3. The preparation method according to claim 1, It is characterized in that The crystallization temperature is 150-240°C.
4. The preparation method according to claim 1, It is characterized in that The crystallization time is 12 to 36 hours.
5. The preparation method according to claim 1, It is characterized in that In the hydrogen / inert gas mixed gas, the volume ratio of hydrogen to inert gas is 1:8-10.
6. The preparation method according to claim 1, It is characterized in that The pH is adjusted to be ≥9.
7. The catalyst prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the catalyst according to claim 7 in the preparation of light olefins by hydrogenation of carbon dioxide.
9. A method for preparing light olefins by hydrogenating carbon dioxide, It is characterized in that Take the catalyst according to claim 7, introduce H 2 and CO 2 The mixed gas is hydrogenated at 280-300°C and 0.1-4MPa.
10. The method according to claim 9, It is characterized in that The H 2 and CO 2 In the mixed gas, H 2 :CO 2 The volume ratio is 3 to 1:1.
Citation Information
Patent Citations
Catalyst for regulating and controlling CO2 hydrogenation target product to be C2-4 olefin, and preparation method of catalyst
CN111215080A
Method for preparing olefin through hydrogenation of carbon dioxide
CN114471560A
Oxidation process for the production of alkenes and carboxylic acids
US20030149295A1