Acid radical salt loaded Mn-based oxide catalyst as well as preparation method and application thereof

Through the Mn-based oxide catalyst supported by the acid salt, combined with the doping of Zr and phosphate, the problems of low CVOCs removal efficiency and insufficient catalyst performance in the prior art are solved, and efficient low-temperature catalytic oxidation performance and stability are achieved. CVOCs removal in multiple industries.

CN118874503AActive Publication Date: 2024-11-01ZHEJIANG UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410914106.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-01
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

The prior art is difficult to effectively remove chlorine-containing volatile organic compounds (CVOCs) in low-temperature catalytic oxidation, and the catalyst lacks oxygen vacancy and acid sites, resulting in poor chlorine poisoning performance and many by-products, affecting industrial applications.

Method used

The Mn-based oxide catalyst supported by acid salt is prepared by the interfacial redox method with rich oxygen vacancies and acid sites. Combined with the doping of Zr and phosphate, the oxidation and acidity of the catalyst are improved and the acidity of the catalyst is enhanced. Low temperature catalytic performance.

Benefits of technology

It achieves a removal efficiency of 90% at 181°C at 10000h-1 airspeed and 500ppm chlorobenzene load, with high specific surface area and stability. It is suitable for CVOCs removal in chlor-alkali industry, pharmaceutical and chemical industries, pesticide and chemical industries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874503A_ABST
    Figure CN118874503A_ABST
Patent Text Reader

Abstract

The invention discloses an acid radical salt loaded Mn-based oxide catalyst and a preparation method and application thereof.According to the acid radical salt loaded Mn-based oxide catalyst, layering of H2O and CH2Cl2 serves as an interface, KMnO4 and Zr (NO3) 4 are dissolved into upper H2O, n-butylamine is slowly injected into lower CH2Cl2, n-butylamine enters a water phase from an organic phase to react in the reaction process, delta-MnO2 is generated on the interface and adsorbed on the surface of delta-MnO2, and the acid radical salt loaded Mn-based oxide catalyst is obtained. Further agglomeration of the product is hindered, and mesoporous delta-MnO2 is formed. In addition, n-butylamine is alkaline, Zr < 4 + > in the upper solution is precipitated in the process of slowly diffusing to the upper solution, and the MnZr oxide catalyst is obtained. And immersing the obtained MnZr catalyst in an (NH) 3PO4 solution, and carrying out centrifugal drying and calcination to obtain the phosphate-loaded MnZr oxide catalyst. The raw materials used in the method are cheap and easy to obtain, and the method is simple and easy to popularize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of preparation methods for highly efficient CVOCs removal catalysts, and in particular to an acid radical-supported Mn-based oxide catalyst and a preparation method thereof, and application in the removal of CVOCs from fixed sources (chlor-alkali industry, pharmaceutical chemical industry, pesticide chemical industry, etc.). Background Art

[0002] With the development of industry, various pollution problems have become increasingly serious, and air pollution is one of them. Chlorinated volatile organic compounds (CVOCs) are major air pollutants, mainly from the use and emission of products containing CVOCs. Low-temperature catalytic oxidation technology is a promising CVOCs control technology due to its advantages such as low reaction temperature, low energy consumption and high safety.

[0003] Generally, the catalytic oxidation process of CVOCs includes four steps: adsorption, activation, Cl dissociation, and deep oxidation. The anti-chlorine poisoning performance depends on the adsorption and dissociation of Cl on the acidic sites. In addition, the form of Cl dissociation plays a crucial role in the generation of polychlorinated by-products. Introducing B acid sites to promote dechlorination in the form of HCl is an effective strategy to inhibit the chlorination of organic compounds and the formation of polychlorinated by-products. Based on the Marse van Krevelen (MvK) mechanism, the catalytic oxidation of VOCs depends largely on the recycling of oxygen species through oxygen vacancies on transition metal oxide catalysts. Therefore, by simultaneously increasing oxygen vacancies and Acid sites, synergistically improving the oxidizability and acidity of transition metal oxides, are effective strategies to enhance the catalytic activity of CB oxidation, resist chlorine poisoning, and inhibit byproducts.

[0004] Manganese-based catalysts have been widely studied as a catalyst for low-temperature CVOC catalytic oxidation. The conversion of Zr can not only promote electron transfer, but also generate oxygen vacancies and promote the migration of oxygen species. Zr, as a cheap and non-toxic transition metal element, has been widely used in various catalyst formulations. The oxygen vacancy content in Mn oxide can be increased by doping with Zr. In addition, the coordination effect between Mn and Zr is beneficial to In addition to bulk doping, the surface loading of phosphate can induce the formation of oxygen vacancies on the surface of Mn oxide through electronic regulation, and the hydroxyl groups introduced by phosphate provide abundant acid sites. Therefore, the synthesis of Mn-based oxide catalysts with acid sites are of great significance for the efficient removal of CVOCs in the chlor-alkali industry, pharmaceutical chemical industry, pesticide chemical industry and other industries. Summary of the invention

[0005] The invention provides an acid radical salt-loaded Mn-based oxide catalyst, a preparation method thereof, and application thereof in removing CVOCs in the chlor-alkali industry, pharmaceutical chemical industry, pesticide chemical industry and other industries.

[0006] The prepared catalyst has high specific surface area, abundant oxygen vacancies and acid sites, which exhibit excellent low-temperature catalytic performance in CVOCs catalytic oxidation (10000h -1 space velocity, under a load of 500ppm chlorobenzene, a removal efficiency of 90% can be achieved at 181°C). At the same time, the raw materials used in the catalyst are cheap and easy to obtain, the preparation method is simple and fast, and it has potential application prospects in the field of CVOCs catalytic oxidation.

[0007] A method for preparing an acid salt-supported Mn-based oxide catalyst comprises the following steps:

[0008] 1) Weigh KMnO4 and metal salt and dissolve them in water, stirring to form solution A;

[0009] Take dichloromethane and record it as solution B;

[0010] Pour solution A into the reactor containing solution B, wait for stratification and interface formation, and place the reactor in a water bath at 20-30℃;

[0011] Inject n-butylamine into the lower layer of dichloromethane in the reactor, let it stand, and a yellow-brown precipitate is generated at the interface. The precipitate is centrifuged, dried, and moved to a muffle furnace, and calcined at 300-400° C. for 2-4 hours in an air atmosphere to obtain a MnZr oxide catalyst;

[0012] 2) dissolving the MnZr oxide catalyst in water, stirring and then ultrasonically dispersing, adding acid salt and stirring, stirring, centrifugally washing with water and drying, transferring to a muffle furnace, and calcining at 300-400° C. for 2-4 hours in an air atmosphere to obtain an acid salt-supported Mn-based oxide catalyst.

[0013] The present invention uses KMnO4 and n-butylamine as raw materials and adopts an interfacial redox method to prepare a mesoporous catalyst with abundant pores and a high specific surface area; the present invention utilizes the alkalinity of n-butylamine to slowly precipitate metal cations in the upper layer while generating delta-MnO2 through redox, thereby preparing a manganese-based composite oxide catalyst with uniform element doping and promoting the formation of oxygen vacancies; the present invention uses acid salts to load the manganese-based composite oxide catalyst, prepares an acid salt-loaded Mn-based oxide catalyst, and promotes the synergistic enhancement of oxygen vacancies and acid sites.

[0014] In step 1), the metal salt is at least one of Zr(NO3)3, Zr(NO3)4, Fe(NO3)3, Sn(NO3)4, and Ni(NO3)2.

[0015] In step 1), the molar ratio of the metal salt to KMnO4 is 1:1-7.

[0016] In step 1), the molar ratio of n-butylamine to KMnO4 is 3 to 7:1.

[0017] In step 1), the standing time is 10-30 hours.

[0018] In step 2), the acid salt is (NH)3PO4·2H2O, (NH4)2SO4, (NH4)6W7O 24 One of 6H2O and (NH4)2MoO4.

[0019] In step 2), the mass ratio of the acid radical salt to the MnZr oxide catalyst is 0.5-2.0:1.

[0020] In step 2), add the acid salt and stir with sealing film for 1-20 hours.

[0021] Furthermore, the specific technical solution of the present invention is as follows:

[0022] Weigh 3.16g (0.02mol) KMnO4, dissolve an appropriate amount of Zr(NO3)4 in 100ml deionized water, and continue stirring for 30min to form solution A; measure 50ml CH2Cl2, record it as solution B. First slowly pour solution B into a 250ml beaker, then slowly pour solution A, let it stand for 5min, wait for stratification, form an interface, and place the beaker in a 25℃ water bath. Weigh 7.314g (0.1mol) n-butylamine, introduce it into a syringe, slowly inject n-butylamine into the lower layer of CH2Cl2, let it stand for 24 hours, and a yellow-brown precipitate will form at the interface. The precipitate is centrifuged and washed with water 6 times, dried at 80℃ for 8 hours, and then moved to a muffle furnace. It is calcined at 350℃ in an air atmosphere for 3 hours to obtain a Mn-based composite oxide catalyst Zr1Mn x , 1 / x represents the molar ratio of Zr(NO3)4 to KMnO4 in different samples. x The oxide catalyst was dissolved in 40 ml of deionized water, stirred for 30 min and then ultrasonically dispersed for 30 min. An appropriate amount of (NH)3PO4·2H2O was weighed and dissolved in the above solution. After stirring for 10 h, the solution was centrifuged and washed with water three times. After drying at 80 ° C for 8 hours, the solution was transferred to a muffle furnace and calcined at 350 ° C for 3 hours in an air atmosphere to obtain a phosphate-supported Mn-based composite oxide catalyst nP-Zr1Mn x, n% represents the P and Zr1Mn in the (NH)3PO4·2H2O feed x Mass ratio of catalyst.

[0023] In the above-mentioned method for preparing the high-performance Mn-based composite oxide catalyst for removing CVOCs at low temperature, the preferred nitrate is Zr(NO3)4, and there is a better synergistic effect between Mn and Zr.

[0024] The preferred molar ratio of Zr(NO3)4 to KMnO4 is: 1 / 5;

[0025] The preferred standing time after the slow injection of n-butylamine is 24 hours. If the time is too short, the reaction will not be complete, and if the time is too long, the product particles will be too large.

[0026] The preferred acid salt is (NH4)3PO4·2H2O. Phosphate has a better control capability on the electrons on the surface of Mn oxide.

[0027] The preferred (NH4)3PO4·2H2O feed amount is 0.98 g. If the feed amount is too little, the phosphate loading is too little; if the feed amount is too much, the loading is excessive.

[0028] The preferred stirring time after dissolving (NH4)3PO4·2H2O is 10 h. If the time is too short, the loading amount is too small, and if the time is too long, the loading amount is excessive.

[0029] A high-performance Mn-based composite oxide catalyst for removing CVOCs at low temperature prepared by the above preparation method.

[0030] The above-mentioned high-performance phosphate-loaded Mn-based composite oxide catalyst for low-temperature removal of CVOCs is used in the application of CVOCs in tail gas from the chlor-alkali industry, pharmaceutical chemical industry, and pesticide chemical industry.

[0031] Compared with the prior art, the present invention has the following advantages:

[0032] 1. The raw materials used are cheap and readily available, the preparation method is simple, the equipment is simple, easy to promote, and can be mass-produced;

[0033] 2. It is a universal method for preparing acid salt-loaded Mn-based composite oxides;

[0034] 3. The manganese-based composite oxide catalyst prepared by this method has the advantages of rich mesoporous structure, high specific surface area, abundant oxygen vacancies, acidic sites, and uniform dispersion of loaded elements, thus showing excellent low-temperature CVOCs catalytic oxidation activity and stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 XRD results of manganese-based composite oxide catalysts.

[0036] Figure 2 The SEM results of manganese-based composite oxide catalysts.

[0037] Figure 3 These are the N2- adsorption and desorption results of the manganese-based composite oxide catalyst.

[0038] Figure 4 This is the EDS result of manganese-based composite oxide catalyst.

[0039] Figure 5 TEM results of manganese-based composite oxide catalysts.

[0040] Figure 6 NH3-TPD results of manganese-based composite oxide catalysts.

[0041] Figure 7 The results are the activity results (removal efficiency) of chlorobenzene catalytic oxidation over manganese-based catalysts.

[0042] Figure 8 These are the stability test results of catalytic oxidation of chlorobenzene by manganese-based catalysts.

[0043] Fig. 9 These are the activity results of 15P-Zr1Mn5 catalyst for catalytic oxidation of dichloromethane, vinyl chloride and ethylene dichloride. DETAILED DESCRIPTION

[0044] Example 1. Preparation of Zr1Mn3 manganese-based catalyst

[0045] Accurately weigh 3.16g (0.02mol) KMnO4 and 2.87g Zr(NO3)4·5H2O and dissolve them in 100ml deionized water, stirring continuously for 30min to form solution A; weigh 50ml CH2Cl2 and record it as solution B. First, slowly pour solution B into a 250ml beaker, then slowly pour solution A into it, let it stand for 5min, wait for stratification and interface formation, and place the beaker in a 25℃ water bath. Weigh 7.314g (0.1mol) n-butylamine, introduce it into a syringe, slowly inject n-butylamine into the lower layer of CH2Cl2, let it stand for 24 hours, and a yellow-brown precipitate will form at the interface. The precipitate will be centrifuged and washed with water for 6 times, dried at 80℃ for 8 hours, and then moved to a muffle furnace and calcined at 350℃ in an air atmosphere for 3 hours to obtain a Mn-based composite oxide catalyst Zr1Mn3. The BET test results show that the specific surface area of ​​the Zr1Mn3 manganese-based composite oxide catalyst prepared with a molar ratio of Zr(NO3)4 to KMnO4 of 1 / 3 reaches 127.7 m 2 / g, the average pore diameter is 10.48nm, and the pore volume reaches 0.314cm 3 / g (as shown in Table 1).

[0046] Example 2: Preparation of Zr1Mn5 manganese-based catalyst

[0047] The mass of Zr(NO3)4·5H2O weighed in Example 1 was changed to 1.72g, and the other conditions remained unchanged to obtain a Mn-based catalyst Zr1Mn5 sample. The BET test results showed that the specific surface area of ​​the Zr1Mn5 manganese-based composite oxide catalyst prepared with a molar ratio of Zr(NO3)4 to KMnO4 of 1 / 5 reached 193.8m 2 / g, the average pore diameter is 5.47nm, and the pore volume reaches 0.474cm 3 / g (as shown in Table 1).

[0048] Example 3. Preparation of Zr1Mn7 manganese-based catalyst

[0049] The mass of Zr(NO3)4·5H2O weighed in Example 1 was changed to 1.23g, and the other conditions remained unchanged to obtain a Mn-based catalyst Zr1Mn7 sample. The BET test results showed that the specific surface area of ​​the Zr1Mn7 manganese-based composite oxide catalyst prepared with a molar ratio of Zr(NO3)4 to KMnO4 of 1 / 7 reached 131.2 m 2 / g, the average pore diameter is 16.58nm, and the pore volume reaches 0.291cm 3 / g (as shown in Table 1).

[0050] Example 4: Preparation of 10P-Zr1Mn5 manganese-based catalyst

[0051] Weigh 1 g of the Zr1Mn5 catalyst obtained in Example 2, dissolve it in 40 ml of deionized water, stir for 30 min, and then disperse it by ultrasonic for 30 min. Weigh 0.65 g of (NH)3PO4·2H2O and dissolve it in the above solution. Stir for 10 h, then centrifuge and wash it with water 3 times. After drying at 80°C for 8 hours, move it to a muffle furnace and calcine it at 350°C in an air atmosphere for 3 hours to obtain 10P-Zr1Mn5 with a P loading of 10%. The BET test results show that the specific surface area of ​​the prepared 10P-Zr1Mn5 catalyst reaches 189.27 m 2 / g, the average pore diameter is 6.63nm, and the pore volume reaches 0.375cm 3 / g (as shown in Table 1).

[0052] Example 5. Preparation of 15P-Zr1Mn5 manganese-based catalyst

[0053] The mass of (NH)3PO4·2H2O weighed in Example 4 was changed to 0.98 g, and the other conditions remained unchanged to obtain 15P-Zr1Mn5 with a P loading of 15%. The BET test results showed that the specific surface area of ​​the prepared 15P-Zr1Mn5 catalyst reached 182.9 m2 / g, the average pore diameter is 6.89nm, and the pore volume reaches 0.347cm 3 / g (as shown in Table 1).

[0054] Example 6: Preparation of 20P-Zr1Mn5 manganese-based catalyst

[0055] The mass of (NH)3PO4·2H2O weighed in Example 4 was changed to 1.30 g, and the other conditions remained unchanged to obtain 20P-Zr1Mn5 with a P loading of 20%. The BET test results showed that the specific surface area of ​​the prepared 15P-Zr1Mn5 catalyst reached 173.2 m 2 / g, the average pore diameter is 7.74nm, and the pore volume reaches 0.335cm 3 / g (as shown in Table 1).

[0056] The XRD results of manganese-based composite oxide catalysts are shown in Figure 1 As shown in the figure, the obtained catalyst presents a δ-MnO2 crystalline phase. As the molar ratio of Zr(NO3)4 to KMnO4 increases, the XRD peak intensity decreases, and as the phosphate loading increases, it gradually tends to an amorphous structure.

[0057] The SEM results of manganese-based composite oxide catalysts are shown in Figure 2 As shown, it can be seen from the figure that the catalyst has a large number of pore structures.

[0058] The results of N2- adsorption and desorption on manganese-based composite oxide catalysts are shown in Figure 3 As shown in the figure, it can be seen that the catalyst has abundant mesopores and Zr doping increases the specific surface area of ​​Mn oxide.

[0059] EDS results of manganese-based composite oxide catalysts are shown in Figure 4 As shown in the figure, it can be seen that the Zr, Mn and P elements of the 15P-Zr1Mn5 catalyst prepared with a molar ratio of Zr(NO3)3 to KMnO4 of 1 / 5 and a phosphate loading of 15% are evenly dispersed. This is because the preparation method of the interface is conducive to the full mixing of Zr and Mn, and the doping of Zr increases the specific surface area of ​​Mn oxide, which is conducive to the uniform loading of phosphate and helps to form a stronger synergistic effect between elements.

[0060] TEM results of manganese-based composite oxide catalysts are shown in Figure 5 As shown in the figure, the yellow T represents lattice distortion, and the green oval box represents lattice defects, indicating that the 15P-Zr1Mn5 catalyst prepared with a molar ratio of Zr(NO3)3 to KMnO4 of 1 / 5 and a phosphate loading of 15% has a large number of lattice defects, indicating the formation of abundant oxygen vacancies.

[0061] The NH3-TPD results of manganese-based composite oxide catalysts are shown in Figure 6 As shown in Figure 2, Zr doping increases the weak acidity of δ-MnO2, and phosphate loading increases the strong acidity of δ-MnO2.

[0062] The results of the activity (removal efficiency) of chlorobenzene catalytic oxidation by manganese-based catalysts are as follows: Figure 7 The stability test results of chlorobenzene catalytic oxidation by manganese-based catalyst are shown in Figure 8 The results of the catalytic oxidation of dichloromethane, vinyl chloride and dichloroethane by 15P-Zr1Mn5 catalyst are shown in Fig. 9 As shown. Figure 7 , 8, 9 It can be seen that the phosphate-loaded manganese-based composite oxide series catalysts have good low-temperature catalytic oxidation activity and stability when catalyzing the oxidation of CVOCs.

[0063] Table 1

[0064]

[0065] The catalysts prepared in Examples 1, 2, 3, 4, 5, and 6 were applied to the catalytic oxidation reaction of CVOCs, and all showed good catalytic activity. The removal efficiency of the catalysts prepared in Examples 1, 2, 3, 4, 5, and 6 was as follows: Figure 6 , as shown in 7. The reaction was carried out on a CVOCs catalytic oxidation evaluation device. The catalyst evaluation device mainly consists of four parts: gas pipeline, fixed bed reactor, flow control system and gas detection system. During the experiment, a mass flow meter was used to achieve precise control of each gas. A quartz tube with an outer diameter of 10 mm and an inner diameter of 6 mm was used as the catalytic reactor. The reactor was heated by a resistance furnace, and the temperature in the reactor was monitored by a K-type thermocouple. The total flow rate of the mixed gas was 50 mL min -1 The volume fraction of O2 is 20%, and the chlorobenzene is controlled to 1000 ml·m by adjusting the flow ratio of two standard air. -3 During the experiment, the catalyst loading was 300 mg, the particle size was 40-60 mesh, and the corresponding mass space velocity (WHSV) was 10000 mL·(g·h) -1 .

Claims

1. A method for preparing an acid salt-supported Mn-based oxide catalyst, characterized in that: The following steps are involved: 1) Weigh KMnO4 and metal salt and dissolve them in water, stirring to form solution A; Take dichloromethane and record it as solution B; Pour solution A into the reactor containing solution B, wait for stratification and interface formation, and place the reactor in a water bath at 20-30℃; Inject n-butylamine into the lower layer of dichloromethane in the reactor, let it stand, and a yellow-brown precipitate is generated at the interface. The precipitate is centrifuged, dried, and moved to a muffle furnace, and calcined at 300-400° C. for 2-4 hours in an air atmosphere to obtain a MnZr oxide catalyst; 2) dissolving the MnZr oxide catalyst in water, stirring and then ultrasonically dispersing, adding acid salt and stirring, stirring, centrifugally washing with water and drying, transferring to a muffle furnace, and calcining at 300-400° C. for 2-4 hours in an air atmosphere to obtain an acid salt-supported Mn-based oxide catalyst.

2. The method for preparing the acid salt-supported Mn-based oxide catalyst according to claim 1, characterized in that: In step 1), the metal salt is at least one of Zr(NO3)3, Zr(NO3)4, Fe(NO3)3, Sn(NO3)4, and Ni(NO3)2.

3. The method for preparing the acid salt-supported Mn-based oxide catalyst according to claim 1, characterized in that: In step 1), the molar ratio of the metal salt to KMnO4 is 1:1-7.

4. The method for preparing the acid salt-supported Mn-based oxide catalyst according to claim 1, characterized in that: In step 1), the molar ratio of n-butylamine to KMnO4 is 3 to 7:

1.

5. The method for preparing the acid salt-supported Mn-based oxide catalyst according to claim 1, characterized in that: In step 1), the standing time is 10-30 hours.

6. The method for preparing the acid salt-supported Mn-based oxide catalyst according to claim 1, characterized in that: In step 2), the acid salt is (NH)3PO4·2H2O, (NH4)2SO4, (NH4)6W7O 24 One of 6H2O and (NH4)2MoO4.

7. The method for preparing the acid salt-supported Mn-based oxide catalyst according to claim 1, characterized in that: In step 2), the mass ratio of the acid radical salt to the MnZr oxide catalyst is 0.5-2.0:

1.

8. The method for preparing the acid salt-supported Mn-based oxide catalyst according to claim 1, characterized in that: In step 2), add the acid salt and stir with sealing film for 1-20 hours.

9. The acid salt-supported Mn-based oxide catalyst prepared according to the preparation method according to any one of claims 1 to 8.

10. Use of the acid salt-supported Mn-based oxide catalyst according to claim 9 in low-temperature removal of CVOCs.

Citation Information

Patent Citations

  • Hydrothermal-resistant composite catalyst as well as preparation method and application thereof

    CN110252285A

  • MnZr catalyst for catalytic oxidation of VOCs, and preparation method and application of MnZr catalyst

    CN111790374A

  • Phosphorylated perovskite type catalyst as well as preparation method and application thereof

    CN112604700A

  • Acid site separation catalyst for synergistic conversion of nitrogen oxides and chlorine-containing volatile organic compounds, and preparation method and application thereof

    CN114308088A

  • Catalyst for catalytic oxidation of dichloromethane and preparation method thereof

    CN114768836A