Catalyst with aerogel as carrier and application of catalyst in methane oxidation
By using an amino-modified carbon aerogel support and Au, Pt, and Pd synergistic catalysts, the problem of low efficiency of existing methane catalysts has been solved, and the preparation of methanol with high selectivity has been achieved, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202411001545.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing catalysts for the catalytic oxidation of methane to methanol have low catalytic efficiency and methanol selectivity, which hinders the industrial application of one-step conversion of methane to methanol.
Using an aerogel-supported catalyst, the loading rate of active nano-metals was improved by carbon aerogel amination modification, and Au, Pt and Pd were used for synergistic catalysis to achieve the direct oxidation of methane to methanol at a lower temperature.
It improves the selectivity and yield of methanol, simplifies the process, reduces reaction costs, and is suitable for industrial application.
Smart Images

Figure BDA0004961705870000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of methane catalytic oxidation, and particularly relates to a catalyst using aerogel as a carrier and application of the catalyst in methane oxidation. Background Art
[0002] Methane (CH4) is one of the most important fossil fuels in the world. It is abundant and widely distributed in natural gas, shale gas, coalbed methane, combustible ice and biogas. It is not only a commonly used fossil fuel, but also an important raw material for the production of high value-added chemicals. Among the many high value-added chemicals produced from methane as raw material, methanol (CH3OH) is not only a liquid fuel that is easy to store and transport, but also a raw material for the preparation of olefins, aromatics and other fine chemicals. Therefore, it is considered to be one of the ideal products of methane conversion. In industry, the method of synthesizing methanol from methane as raw material is an indirect method, that is, methane is first converted into synthesis gas (a mixture of carbon monoxide and hydrogen) through steam reforming under high temperature and high pressure conditions. Then, the synthesis gas is converted into methanol through Fischer-Tropsch synthesis. This method has problems such as complicated process flow, high energy consumption and high reaction cost, which seriously hinders its sustainable development.
[0003] The direct method of converting methane into methanol in one step can greatly simplify the process and reduce the reaction cost. However, in the reaction process of direct conversion of methane to methanol, since methanol molecules are more active than methane molecules, the product methanol is easily over-oxidized to produce carbon monoxide and carbon dioxide. Therefore, a suitable catalyst is needed to suppress the peroxidation reaction of methanol in the direct conversion of methane and achieve its directional conversion. There are many catalysts for the catalytic oxidation of methane to prepare formaldehyde, but there are generally problems of low catalytic efficiency and methanol selectivity, which hinders the industrial application of one-step conversion of methane to methanol. Summary of the invention
[0004] In order to solve the deficiencies mentioned in the above background technology, the purpose of the present invention is to provide a catalyst with aerogel as a carrier and its application in methane oxidation. The loading rate of active nanometals in the aerogel carrier is increased by amino modification of carbon aerogel, and the direct oxidation of methane to produce methanol can be achieved at a lower temperature through the synergistic catalysis of Au, Pt and Pd, and the selectivity of methanol is high.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A catalyst with aerogel as a carrier, the catalyst consists of an aerogel carrier and an active component loaded on the carrier, the aerogel carrier is an amino-modified carbon aerogel, the active component comprises nano Au, nano Pt and nano Pd, the loading amount of Au is 3-6wt% of the carrier mass, the loading amount of Pt is 5-12wt% of the carrier mass, and the loading amount of Pd is 12-25wt% of the carrier mass;
[0007] The preparation method of the catalyst comprises the following steps:
[0008] S1, dissolving chloroauric acid, chloroplatinic acid and palladium chloride in a mixed solution of ethanol and ethylene glycol to obtain a precursor solution;
[0009] S2, add aerogel carrier to the precursor solution in a certain proportion, ultrasonically treat for 20 to 40 minutes, and 3+ , Pt 4 + , Pd 2+ Adsorbed on aerogel carrier;
[0010] S3, adding a reducing agent, reacting at 105-115°C for 2-4 hours. After the reaction is completed, filtering by micropore, washing with acetone and water, and vacuum drying for 12 hours to prepare a catalyst.
[0011] Further preferably, in step S1, the molar ratio of chloroauric acid, chloroplatinic acid and palladium chloride is 1:1-2:2-5, and the molar concentration of chloroauric acid in the precursor solution is 0.10-0.15 mol / L.
[0012] Further preferably, in step S1, ethanol and ethylene glycol are mixed in a volume ratio of 1:1 to 3.
[0013] Further preferably, the reducing agent is one of NaBH4, KBH4, LiBH4, hydrazine hydrate and sodium citrate.
[0014] Further preferably, the method for preparing the aerogel carrier comprises the following steps:
[0015] (1) a certain amount of resorcinol and formaldehyde are mixed and dissolved, and PEG-2000 is added and mixed uniformly to obtain solution A, and then a certain amount of white oil is taken, diglycerol dioleate is added to the white oil, and the mixture is stirred uniformly to obtain solution B;
[0016] (2) Pour solution A into solution B, emulsify for 4 to 6 minutes using a high shear dispersing emulsifier, stir and heat to 60° C. for reaction for 8 to 12 hours to obtain hydrogel microspheres, wash with dichloromethane and dry to obtain organic aerogel, then place the organic aerogel in a tubular furnace and obtain carbon aerogel through a carbonization process;
[0017] (3) adding a certain amount of 3-aminopropyltriethoxysilane to toluene and stirring uniformly to obtain a 3-aminopropyltriethoxysilane solution, adding the carbon aerogel in step (2) to the 3-aminopropyltriethoxysilane solution at a solid-liquid ratio of 1:8-10, reflux at 80° C. for 12-24 h, then washing with toluene and n-hexane to remove the residual solvent on the surface, and finally drying to obtain the amino-modified carbon aerogel.
[0018] Further preferably, the molar ratio of resorcinol to formaldehyde is 1:2, and the amount of PEG-2000 added is 2% of the mass of resorcinol.
[0019] More preferably, the volume of the white oil is 3 times the volume of solution A, and the content of dipolyglycerol dioleate is 1.5 wt % of the total mass of the white oil.
[0020] Further preferably, the carbonization process in step (2) is specifically as follows: the organic aerogel is heated to 900°C at a rate of 5°C / min, carbonized at high temperature for 3 to 5 hours, then cooled to 880°C, a CO2 activator is introduced, and activated for 8 to 12 hours to obtain a high specific surface area carbon aerogel.
[0021] Further preferably, 3-aminopropyltriethoxysilane and toluene are mixed in a volume ratio of 1:10.
[0022] A catalyst with aerogel as carrier is used in methane oxidation. In aqueous solution, hydrogen / oxygen mixed gas is used as oxidant, and methane is directly oxidized by the catalyst at 50-60°C to prepare methanol. The selectivity of methanol is ≥90%.
[0023] Beneficial effects of the present invention:
[0024] The catalyst with aerogel as carrier of the present invention is composed of an aerogel carrier and an active component loaded on the carrier, wherein the aerogel carrier is an amino-modified carbon aerogel, and the interior and surface of the carbon aerogel are enriched with amino groups by amination modification of resorcinol and formaldehyde-based carbon aerogel by 3-aminopropyltriethoxysilane, thereby improving the adsorption capacity of the carbon aerogel for metal ions, thereby improving the loading rate of active nano metals in the aerogel carrier. The active components of the present invention include nano Au, nano Pt and nano Pd, and through the coordinated catalysis of Au, Pt and Pd, direct oxidation of methane to prepare methanol can be achieved at a relatively low temperature, the process conditions are simple, the selectivity of methanol is high, and it is suitable for industrial promotion and application. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Example 1
[0027] A method for preparing an aerogel carrier comprises the following steps:
[0028] (1) 85 ml of resorcinol and 60 ml of formaldehyde were mixed and dissolved, and 40 g of PEG-2000 was added and mixed uniformly to obtain solution A. 440 ml of white oil was then taken, and 5.6 g of diglycerol dioleate was added to the white oil, and the mixture was stirred uniformly to obtain solution B;
[0029] (2) Pour solution A into solution B, emulsify with a high shear dispersing emulsifier for 5 min, stir and heat to 60 ° C for 10 h to obtain hydrogel microspheres, wash with dichloromethane and dry to obtain organic aerogel, then put the organic aerogel into a tubular furnace, heat to 900 ° C at a rate of 5 ° C / min, high temperature carbonize for 4 h, then cool to 880 ° C, introduce CO2 activator, activate for 10 h, and obtain high specific surface area carbon aerogel;
[0030] (3) 3-aminopropyltriethoxysilane and toluene are mixed in a volume ratio of 1:10 to obtain a 3-aminopropyltriethoxysilane solution, and the carbon aerogel in step (2) is added to the 3-aminopropyltriethoxysilane solution in a solid-liquid ratio of 1:9, and refluxed at 80° C. for 18 h, then washed with toluene and n-hexane to remove the residual solvent on the surface, and finally dried to obtain the amino-modified carbon aerogel.
[0031] Example 2
[0032] A catalyst with an aerogel as a carrier, the catalyst comprising an aerogel carrier and active components loaded on the carrier, the aerogel carrier is the amino-modified carbon aerogel prepared in Example 1, and the active components include nano-Au, nano-Pt and nano-Pd.
[0033] The preparation method of the catalyst comprises the following steps:
[0034] S1, dissolving 3.4 g of chloroauric acid, 8.1 g of chloroplatinic acid and 3.5 g of palladium chloride in a mixed solution of ethanol and ethylene glycol to obtain a precursor solution;
[0035] S2, add aerogel carrier into the precursor solution in a certain proportion, ultrasonically treat for 30 minutes, and 3+ , Pt 4+ , Pd2 + Adsorbed on aerogel carrier;
[0036] S3, adding a reducing agent, reacting at 110° C. for 3 h, after the reaction is completed, microporous filtration, washing with acetone and water, and vacuum drying for 12 h to prepare the catalyst.
[0037] According to detection, the loading amount of Au in the above catalyst is 5.1wt% of the carrier mass, the loading amount of Pt is 11.5wt% of the carrier mass, and the loading amount of Pd is 12.3wt% of the carrier mass.
[0038] Example 3
[0039] A catalyst with an aerogel as a carrier, the catalyst comprising an aerogel carrier and active components loaded on the carrier, the aerogel carrier is the amino-modified carbon aerogel prepared in Example 1, and the active components include nano-Au, nano-Pt and nano-Pd.
[0040] The preparation method of the catalyst comprises the following steps:
[0041] S1, dissolving 3.5 g of chloroauric acid, 4.0 g of chloroplatinic acid and 3.5 g of palladium chloride in a mixed solution of ethanol and ethylene glycol to obtain a precursor solution;
[0042] S2, add aerogel carrier into the precursor solution in a certain proportion, ultrasonically treat for 20 minutes, and 3+ , Pt 4+ , Pd 2 + Adsorbed on aerogel carrier;
[0043] S3, adding a reducing agent, reacting at 115° C. for 2 h, after the reaction is completed, microporous filtration, washing with acetone and water, and vacuum drying for 12 h to prepare the catalyst.
[0044] According to detection, the loading amount of Au in the above catalyst is 5.8wt% of the carrier mass, the loading amount of Pt is 5.5wt% of the carrier mass, and the loading amount of Pd is 13.6wt% of the carrier mass.
[0045] Example 4
[0046] A catalyst with an aerogel as a carrier, the catalyst comprising an aerogel carrier and active components loaded on the carrier, the aerogel carrier is the amino-modified carbon aerogel prepared in Example 1, and the active components include nano-Au, nano-Pt and nano-Pd.
[0047] The preparation method of the catalyst comprises the following steps:
[0048] S1, dissolving 3.4 g of chloroauric acid, 8.1 g of chloroplatinic acid and 8.8 g of palladium chloride in a mixed solution of ethanol and ethylene glycol to obtain a precursor solution;
[0049] S2, add aerogel carrier to the precursor solution in a certain proportion, ultrasonically treat for 40 minutes, and 3+ , Pt 4+ , Pd 2 + Adsorbed on aerogel carrier;
[0050] S3, adding a reducing agent, reacting at 105° C. for 4 hours, after the reaction is completed, microporous filtration, washing with acetone and water, and vacuum drying for 12 hours to prepare the catalyst.
[0051] According to detection, the loading amount of Au in the above catalyst is 3.3wt% of the carrier mass, the loading amount of Pt is 10.5wt% of the carrier mass, and the loading amount of Pd is 23.9wt% of the carrier mass.
[0052] Example 5
[0053] A catalyst with an aerogel as a carrier, the catalyst comprising an aerogel carrier and active components loaded on the carrier, the aerogel carrier is the amino-modified carbon aerogel prepared in Example 1, and the active components include nano-Au, nano-Pt and nano-Pd.
[0054] The preparation method of the catalyst comprises the following steps:
[0055] S1, dissolving 3.4 g of chloroauric acid, 4.0 g of chloroplatinic acid and 8.8 g of palladium chloride in a mixed solution of ethanol and ethylene glycol to obtain a precursor solution;
[0056] S2, add aerogel carrier to the precursor solution in a certain proportion, ultrasonically treat for 40 minutes, and 3+ , Pt 4+ , Pd 2 + Adsorbed on aerogel carrier;
[0057] S3, adding a reducing agent, reacting at 115° C. for 4 hours, after the reaction is completed, microporous filtration, washing with acetone and water, and vacuum drying for 12 hours to prepare the catalyst.
[0058] According to detection, the loading amount of Au in the above catalyst is 3.5wt% of the carrier mass, the loading amount of Pt is 6.8wt% of the carrier mass, and the loading amount of Pd is 24.7wt% of the carrier mass.
[0059] Comparative Example 1
[0060] A catalyst with aerogel as a carrier, the catalyst consists of an aerogel carrier and active components loaded on the carrier, the aerogel carrier is unmodified resorcinol-formaldehyde based carbon aerogel, and the active components include nano-Au, nano-Pt and nano-Pd.
[0061] The preparation method of the catalyst comprises the following steps:
[0062] S1, dissolving 3.4 g of chloroauric acid, 4.0 g of chloroplatinic acid and 8.8 g of palladium chloride in a mixed solution of ethanol and ethylene glycol to obtain a precursor solution;
[0063] S2, add aerogel carrier to the precursor solution in a certain proportion, ultrasonically treat for 40 minutes, and 3+ , Pt 4+ , Pd 2 + Adsorbed on aerogel carrier;
[0064] S3, adding a reducing agent, reacting at 115° C. for 4 hours, after the reaction is completed, microporous filtration, washing with acetone and water, and vacuum drying for 12 hours to prepare the catalyst.
[0065] According to detection, the loading amount of Au in the above catalyst is 1.4wt% of the carrier mass, the loading amount of Pt is 2.3wt% of the carrier mass, and the loading amount of Pd is 9.8wt% of the carrier mass.
[0066] Comparative Example 2
[0067] A catalyst using an aerogel as a carrier, the catalyst comprising an aerogel carrier and an active component loaded on the carrier, the aerogel carrier is the amino-modified carbon aerogel prepared in Example 1, and the active component is nano-Au.
[0068] The preparation method of the catalyst comprises the following steps:
[0069] S1, dissolving 3.4 g of chloroauric acid in a mixed solution of ethanol and ethylene glycol to obtain a precursor solution;
[0070] S2, add aerogel carrier to the precursor solution in a certain proportion, ultrasonically treat for 40 minutes, and 3+ , Pt 4+ , Pd 2 + Adsorbed on aerogel carrier;
[0071] S3, adding a reducing agent, reacting at 115° C. for 4 hours, after the reaction is completed, microporous filtration, washing with acetone and water, and vacuum drying for 12 hours to prepare the catalyst.
[0072] According to the test, the Au loading in the above catalyst is 13.6 wt% of the carrier mass.
[0073] Comparative Example 3
[0074] A catalyst with an aerogel as a carrier, the catalyst comprising an aerogel carrier and an active component loaded on the carrier, the aerogel carrier is the amino-modified carbon aerogel prepared in Example 1, and the active component is nano-Pt.
[0075] The preparation method of the catalyst comprises the following steps:
[0076] S1, dissolving 4.0 g of chloroplatinic acid in a mixed solution of ethanol and ethylene glycol to obtain a precursor solution;
[0077] S2, add aerogel carrier to the precursor solution in a certain proportion, ultrasonically treat for 40 minutes, and 3+ , Pt 4+ , Pd 2 + Adsorbed on aerogel carrier;
[0078] S3, adding a reducing agent, reacting at 115° C. for 4 hours, after the reaction is completed, microporous filtration, washing with acetone and water, and vacuum drying for 12 hours to prepare the catalyst.
[0079] According to the test, the Pt loading in the above catalyst is 16.3 wt% of the carrier mass.
[0080] Comparative Example 4
[0081] A catalyst with an aerogel as a carrier, the catalyst comprising an aerogel carrier and an active component loaded on the carrier, the aerogel carrier is the amino-modified carbon aerogel prepared in Example 1, and the active component is nano-Pd.
[0082] The preparation method of the catalyst comprises the following steps:
[0083] S1, dissolving 3.5 g of palladium chloride in a mixed solution of ethanol and ethylene glycol to obtain a precursor solution;
[0084] S2, add aerogel carrier to the precursor solution in a certain proportion, ultrasonically treat for 40 minutes, and 3+ , Pt 4+ , Pd 2 + Adsorbed on aerogel carrier;
[0085] S3, adding a reducing agent, reacting at 115° C. for 4 hours, after the reaction is completed, microporous filtration, washing with acetone and water, and vacuum drying for 12 hours to prepare the catalyst.
[0086] According to the test, the Pd loading in the above catalyst is 14.5wt% of the carrier mass.
[0087] Performance Testing
[0088] Examples 2 to 5 were respectively added to a 0.15 mol / L H2O2 aqueous solution and ultrasonically dispersed, and then a stabilizer polyvinyl pyrrolidone was added and stirred to dissolve. At 55°C and 2.5 MPa, CH4 was mixed with H2, O2 and N2 at volume percentages of 75.86%, 0.86%, 1.72% and 21.55%, and then introduced into the H2O2 aqueous solution at a rate of 30 mL / min for catalytic oxidation to prepare methanol. The contents of methanol and by-products in the product were measured, and the methanol selectivity and yield were calculated. The data obtained are shown in Table 1 below.
[0089] Table 1 Test results of catalyst catalytic methane oxidation performance
[0090]
[0091] As can be seen from Table 1, in Examples 2 to 5, the catalyst of the present invention with aerogel as a carrier has a methanol selectivity greater than 90% and a high methanol yield in the process of preparing methanol by catalytic oxidation of methane. In Comparative Example 1, the carbon aerogel was not amino-modified, so the loading rate of the active component was low, the methanol selectivity was slightly reduced, and the methanol yield decreased significantly. In Comparative Examples 2 to 4, a single metal was used for complex reaction, and its catalytic performance was greatly reduced, indicating that the composite metal in the catalyst of the present invention has a synergistic effect in the process of catalytic oxidation of methane to prepare methanol.
[0092] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0093] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A catalyst with aerogel as carrier, characterized in that: The catalyst is composed of an aerogel carrier and an active component loaded on the carrier, wherein the aerogel carrier is an amino-modified carbon aerogel, and the active component includes nano Au, nano Pt and nano Pd, wherein the loading amount of Au is 3-6wt% of the carrier mass, the loading amount of Pt is 5-12wt% of the carrier mass, and the loading amount of Pd is 12-25wt% of the carrier mass; The preparation method of the catalyst comprises the following steps: S1, dissolving chloroauric acid, chloroplatinic acid and palladium chloride in a mixed solution of ethanol and ethylene glycol to obtain a precursor solution; S2, add aerogel carrier to the precursor solution in a certain proportion, ultrasonically treat for 20 to 40 minutes, and 3+ , Pt 4+ , Pd 2 + Adsorbed on aerogel carrier; S3, adding a reducing agent, reacting at 105-115° C. for 2-4 hours, after the reaction is completed, microporous filtration, washing with acetone and water, and vacuum drying for 12 hours to prepare the catalyst.
2. The catalyst with aerogel as carrier according to claim 1, characterized in that: In step S1, the molar ratio of chloroauric acid, chloroplatinic acid and palladium chloride is 1:1-2:2-5, and the molar concentration of chloroauric acid in the precursor solution is 0.10-0.15 mol / L.
3. The catalyst with aerogel as carrier according to claim 1, characterized in that: In the step S1, ethanol and ethylene glycol are mixed in a volume ratio of 1:1 to 3.
4. The catalyst with aerogel as carrier according to claim 1, characterized in that: The reducing agent is one of NaBH4, KBH4, LiBH4, hydrazine hydrate and sodium citrate.
5. The catalyst with aerogel as carrier according to claim 1, characterized in that: The preparation method of the aerogel carrier comprises the following steps: (1) a certain amount of resorcinol and formaldehyde are mixed and dissolved, and PEG-2000 is added and mixed uniformly to obtain solution A, and then a certain amount of white oil is taken, diglycerol dioleate is added to the white oil, and the mixture is stirred uniformly to obtain solution B; (2) Pour solution A into solution B, emulsify for 4 to 6 minutes using a high shear dispersing emulsifier, stir and heat to 60° C. for reaction for 8 to 12 hours to obtain hydrogel microspheres, wash with dichloromethane and dry to obtain organic aerogel, then place the organic aerogel in a tubular furnace and obtain carbon aerogel through a carbonization process; (3) adding a certain amount of 3-aminopropyltriethoxysilane to toluene and stirring uniformly to obtain a 3-aminopropyltriethoxysilane solution, adding the carbon aerogel in step (2) to the 3-aminopropyltriethoxysilane solution at a solid-liquid ratio of 1:8-10, reflux at 80° C. for 12-24 h, then washing with toluene and n-hexane to remove the residual solvent on the surface, and finally drying to obtain the amino-modified carbon aerogel.
6. The catalyst with aerogel as carrier according to claim 1, characterized in that: The molar ratio of resorcinol to formaldehyde is 1:2, and the added amount of PEG-2000 is 2% of the mass of resorcinol.
7. The catalyst with aerogel as carrier according to claim 1, characterized in that: The volume of the white oil is 3 times the volume of solution A, and the dipolyglycerol dioleate is 1.5 wt % of the total mass of the white oil.
8. The catalyst with aerogel as carrier according to claim 1, characterized in that: The carbonization process in step (2) is specifically as follows: heating the organic aerogel to 900°C at a rate of 5°C / min, high-temperature carbonization for 3 to 5 hours, then cooling to 880°C, introducing a CO2 activator, and activating for 8 to 12 hours to obtain a high specific surface area carbon aerogel.
9. The catalyst with aerogel as carrier according to claim 1, characterized in that: The 3-aminopropyltriethoxysilane and toluene are mixed in a volume ratio of 1:
10.
10. Use of the catalyst with aerogel as carrier in methane oxidation according to any one of claims 1 to 9, characterized in that: In aqueous solution, with O2 and H2O2 as oxidants and polyvinyl pyrrolidone as a stabilizer, methane is directly oxidized by the catalyst at 50-60°C to prepare methanol, and the selectivity of methanol is ≥90%.