Application of calcium-containing gangue inhibitor thiodisuccinic acid in scheelite flotation
By using thiodisuccinic acid and sodium oleate as inhibitors and collectors in sedratite flotation, the problem of difficult removal of calcium-containing gangue in sedratite is solved, and an efficient and environmentally friendly sedratite is achieved. Resource utilization reduces mineral processing costs and environmental pollution.
Patent Information
- Application Number
- CN202411099512.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art is difficult to effectively remove calcium-containing ganglite in sedrael flotation, resulting in low resource utilization efficiency. Commonly used inhibitors such as water glass have high energy consumption, large dose of agents, serious environmental pollution, and complex preparation process.
Thiodisuccinic acid is used as an inhibitor and sodium oleate is used as a collector. Through its chelation with calcite and fluorite, the hydrophilicity of mineral surface is enhanced, and the ability of sedrophyte and calcium-containing ganglite is expanded. Floating difference, achieving effective separation.
It significantly reduces the dosage of medicine, improves the recovery rate of sedraelite, reduces wastewater treatment problems, and has a simple and environmentally friendly process, which is suitable for industrial applications.
Smart Images

Figure CN118874694A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of scheelite flotation, and in particular relates to application of thiodisuccinic acid, a calcium-containing gangue inhibitor, in scheelite flotation. Background Art
[0002] As an important strategic metal, tungsten has excellent properties such as high density, high melting point, strong hardness and good wear resistance. It is widely used in aerospace, military industry, machinery, construction, electronics, chemical industry and other fields, and has the reputation of "industrial teeth". my country has rich reserves of tungsten ore resources, mainly wolframite and scheelite. Wolframite resources have the characteristics of high tungsten grade, relatively simple mineral composition, easy mining and high recovery rate. Wolframite is the first choice in the early development and utilization of tungsten resources. However, with the continuous advancement of my country's industrialization process, the consumption of tungsten resources has increased year by year, and the easy-to-mine wolframite resources are almost exhausted. The rational development and utilization of "poor, fine and mixed" scheelite resources is imminent. Calcium-containing minerals such as calcite and fluorite are the main components of the gangue minerals in scheelite. Because they have the same active site atoms (calcium atoms) on the surface of scheelite and similar floatability, they are difficult to be effectively removed in the flotation enrichment process of scheelite, which seriously affects the efficient utilization of scheelite resources. At present, the industry mainly uses water glass as an inhibitor to effectively remove calcium gangue from scheelite. However, when water glass is used as an inhibitor, it usually needs to be combined with heating operation, which consumes a lot of process energy and has poor economic efficiency. In addition, when water glass is used as an inhibitor, there are still problems such as poor inhibition selectivity, large dosage of reagents, and difficult tailings treatment.
[0003] Patent document No. 202210515658.0 discloses an inhibitor for separating scheelite from calcium-containing minerals. The inhibitor is Al 3+ , Fe 3+ 、Ni 2+ , Er 3+ ,La 3+ , Y 3+ 、Ti 4+ 、Zn 2+The chloride, nitrate or sulfate solution of metal ions and quinic acid solution are reacted in a certain ratio in a specific pH environment and temperature environment for a certain period of time to obtain the product. Although the addition of the inhibitor can effectively separate scheelite from calcium-containing gangue, the preparation conditions of the agent are strict, the process is complicated, and the cycle is long. At the same time, the agent needs to be combined with the addition of activators such as lead nitrate and aluminum sulfate during use, which has the disadvantages of complex process operation, large environmental pollution, and large dosage of the agent. The patent document with application number 201710729061.5 discloses a scheelite flotation inhibitor and its preparation process. The inhibitor is prepared by mixing 40% liquid sodium silicate, 20% sulfuric acid, 15% copper sulfate, 10% carboxymethyl cellulose and 15% lead nitrate. Although the agent can effectively reduce the amount of flotation inhibitor added and reduce the amount of tailings backwater treated, the agent still has problems such as weak inhibition selectivity, complex preparation process, and large environmental pollution, which is not conducive to large-scale promotion and application.
[0004] Therefore, how to provide a new type of environmentally friendly and efficient calcium-containing gangue mineral inhibitor to achieve efficient removal of calcium-containing gangue in scheelite is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention
[0005] In order to solve the above technical problems, the present invention proposes the application of sulfodisuccinic acid, a calcium-containing gangue inhibitor, in the flotation of scheelite.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] The invention discloses an application of thiodisuccinic acid as a calcium-containing gangue inhibitor in the flotation of scheelite.
[0008] A scheelite flotation method comprises crushing, grinding, slurry adjustment and flotation. In the flotation process, sulfodisuccinic acid is used as an inhibitor and sodium oleate is used as a collector.
[0009] Beneficial effects: The present invention utilizes the selective adsorption of the inhibitor sulfodisuccinic acid on the surface of calcite and fluorite minerals under the collector sodium oleate system to increase the hydrophilicity of the mineral surface, expand the floatability difference between calcite, fluorite and scheelite, and realize the effective separation of scheelite and calcium-containing gangue. The calcium-containing gangue inhibitor sulfodisuccinic acid provided by the present invention shows good selective inhibition on calcite and fluorite. The sulfodisuccinic acid molecule has abundant carboxyl groups, which can strongly chelate with the calcium ions on the surface of calcite and fluorite minerals and adsorb on the mineral surface, thereby enhancing its hydrophilicity. However, since the tungstate on the surface of scheelite has a larger group size than fluorine and carbonate, the steric hindrance effect is greater when the inhibitor sulfodisuccinic acid chelates with the calcium ions on the surface of scheelite. The inhibitor sulfodisuccinic acid is difficult to adsorb on the surface of scheelite and does not inhibit the flotation of scheelite. Therefore, the addition of the inhibitor thiodisuccinic acid in the present invention can achieve effective removal of fluorite and calcite while ensuring a high recovery rate of scheelite.
[0010] Preferably, the flotation includes one roughing selection, two cleaning selections and one scavenging selection.
[0011] Preferably, sulfodisuccinic acid and sodium oleate are added in the roughing process, and based on the mass of the original ore, the added amount of sulfodisuccinic acid is 60-100 g / t, and the added amount of sodium oleate is 200-400 g / t.
[0012] Beneficial effects: When thiodisuccinic acid is used as an inhibitor, the dosage of the agent is only 60-100 g / t, which can greatly reduce the dosage of the agent compared to the conventional water glass inhibitor (6-10 kg / t), reduce the inhibitory effect on the flotation of the useful mineral scheelite, and alleviate the problems of wastewater purification and return water utilization.
[0013] Preferably, sulfodisuccinic acid is added during the concentration process, and the added amount of sulfodisuccinic acid is 30-50 g / t based on the mass of the original ore.
[0014] Preferably, sodium oleate is added during the scavenging process, and the amount of sodium oleate added is 100-200 g / t based on the mass of the original ore.
[0015] Preferably, the sulfosuccinic acid and sodium oleate are added in the form of solutions;
[0016] Wherein, the mass concentration of thiodisuccinic acid solution is 1%;
[0017] The mass concentration of the sodium oleate solution is 1%.
[0018] Preferably, the slurry preparation is to mix the scheelite powder obtained after grinding with an alkaline solution and water to prepare scheelite slurry.
[0019] Preferably, the alkaline solution is a sodium carbonate solution or a sodium bicarbonate solution with a mass concentration of 1%.
[0020] Preferably, in the scheelite slurry, the mass concentration of scheelite is 15-30%, and the pH value is 7.0-10.5.
[0021] More preferably, the crushing is to use a laboratory small jaw crusher to crush the scheelite ore into particles with a size of less than 2 mm.
[0022] The grinding is to grind the crushed scheelite powder by a ceramic ball mill until the content of particles with a particle size of less than 74 μm accounts for 75% to 85% of the total mass of the scheelite.
[0023] Compared with the prior art, the present invention has the following advantages and technical effects:
[0024] The invention provides an application of thiodisuccinic acid, a calcium-containing gangue inhibitor, in the flotation of scheelite. The invention uses thiodisuccinic acid as an inhibitor to flotate scheelite, and has the characteristics of small dosage of reagents, strong selective inhibition performance, small environmental pollution, easy commercial acquisition, convenient operation and use, etc., and can significantly improve the removal effect of calcium-containing gangue in scheelite, and can greatly reduce the mineral processing cost, so as to facilitate industrial application practice. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0026] Figure 1 It is a process flow chart of scheelite flotation in an embodiment of the present invention. DETAILED DESCRIPTION
[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0029] like Figure 1 As shown, the embodiment of the present invention discloses an application of sulfodisuccinic acid, a calcium-containing gangue inhibitor, in the flotation of scheelite, wherein the flotation comprises one roughing operation, two cleaning operations and one scavenging operation, and specifically comprises the following steps:
[0030] (1) Crushing: Use a laboratory small jaw crusher to crush the scheelite ore to a particle size of <2 mm.
[0031] (2) Grinding: The crushed scheelite powder is finely ground in a ceramic ball mill until the content of particles with a particle size of <74μm accounts for 75-85% of the total mass of the scheelite.
[0032] (3) Slurry preparation: the finely ground scheelite powder is placed in an aerated hanging tank flotation machine, deionized water and a sodium carbonate or sodium bicarbonate solution with a mass concentration of 1% are added thereto, and the mixture is mixed and slurried at a stirring speed of 1992 r / min to obtain a scheelite slurry with a pH value of 7.0 to 10.5 and a scheelite mass concentration of 15 to 30%;
[0033] (4) Flotation: Under room temperature, the scheelite slurry after slurry adjustment is introduced into the flotation machine for one roughing, two cleaning and one scavenging operation. In the roughing process, the inhibitor sulfodisuccinic acid solution and the collector sodium oleate solution are added in sequence, and the addition amount is 60-100g sulfodisuccinic acid and 200-400g sodium oleate per ton of raw ore; the sulfodisuccinic acid solution is added in the cleaning process, and the addition amount is 30-50g sulfodisuccinic acid per ton of raw ore; the sodium oleate solution is added in the scavenging process, and the addition amount is 100-200g sodium oleate per ton of raw ore. The mass concentration of sulfodisuccinic acid solution and sodium oleate solution is 1%. The interval of adding reagents in the flotation process is 3min, and the scraping time is 5min.
[0034] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources;
[0035] Among them, the scheelite in the embodiment of the present invention is taken from a place in Hunan. After chemical multi-element analysis and phase analysis, it can be known that the WO3 content in the ore is 0.52%, the CaO content is 19.35%, and it is a scheelite-calcite type ore, in which the gangue minerals are mainly calcite and quartz, and there is a small amount of fluorite. The scheelite is a typical high-calcium scheelite, and the scheelite is difficult to separate from the calcite and fluorite;
[0036] The inhibitor sulfodisuccinic acid and the collector sodium oleate were both industrially pure, and the pH adjusters sodium carbonate and sodium bicarbonate were chemically pure.
[0037] Unless otherwise specified, the normal temperature or room temperature described in the embodiments of the present invention refers to 25±3°C.
[0038] Example 1
[0039] An application of thiodisuccinic acid, a calcium-containing gangue inhibitor, in the flotation of scheelite specifically comprises the following steps:
[0040] (1) Crushing: Use a laboratory small jaw crusher to crush the scheelite ore to a particle size of <2 mm.
[0041] (2) Grinding: The crushed scheelite powder is finely ground by a ceramic ball mill until the content of particles with a particle size of <74μm accounts for 80% of the total mass of the scheelite.
[0042] (3) Slurry preparation: the finely ground scheelite powder is placed in an aerated hanging tank flotation machine, deionized water and a sodium carbonate solution with a mass concentration of 1% are added thereto, and the mixture is mixed and slurried at a stirring speed of 1992 r / min to obtain a scheelite slurry with a pH value of 7.0 and a scheelite mass concentration of 20%;
[0043] (4) Flotation: Under room temperature, the scheelite slurry after slurry adjustment is introduced into the flotation machine for one roughing, two cleaning and one scavenging operation. In the roughing process, the inhibitor sulfodisuccinic acid solution and the collector sodium oleate solution are added in sequence, and the addition amount is 60g sulfodisuccinic acid and 200g sodium oleate per ton of raw ore; the sulfodisuccinic acid solution is added in the cleaning process, and the addition amount is 30g sulfodisuccinic acid per ton of raw ore; the sodium oleate solution is added in the scavenging process, and the addition amount is 100g sodium oleate per ton of raw ore. The mass concentration of sulfodisuccinic acid solution and sodium oleate solution is 1%. The interval of adding reagents in the flotation process is 3min, and the scraping time is 5min.
[0044] Example 2
[0045] The application of sulfodisuccinic acid, a calcium-containing gangue inhibitor, in the flotation of scheelite is different from that of Example 1 only in that:
[0046] The pH value of the scheelite slurry in step (3) is 9.0.
[0047] The other process steps and parameters are the same as those in Example 1.
[0048] Example 3
[0049] The application of sulfodisuccinic acid, a calcium-containing gangue inhibitor, in the flotation of scheelite is different from that of Example 1 only in that:
[0050] The pH value of the scheelite slurry in step (3) is 11.5.
[0051] The other process steps and parameters are the same as those in Example 1.
[0052] Example 4
[0053] The application of sulfodisuccinic acid, a calcium-containing gangue inhibitor, in the flotation of scheelite is different from that of Example 2 only in that:
[0054] In step (4), the amount of inhibitor added during the roughing process is 80 g / t based on the weight of the original ore;
[0055] The amount of inhibitor added during the concentration process is 40g / t.
[0056] The other process steps and parameters are the same as those in Example 2.
[0057] Example 5
[0058] The application of sulfodisuccinic acid, a calcium-containing gangue inhibitor, in the flotation of scheelite is different from that of Example 2 only in that:
[0059] In step (4), the amount of inhibitor added during the roughing process is 100 g / t based on the weight of the original ore;
[0060] The amount of inhibitor added during the concentration process is 50g / t.
[0061] The other process steps and parameters are the same as those in Example 2.
[0062] Example 6
[0063] The application of sulfodisuccinic acid, a calcium-containing gangue inhibitor, in the flotation of scheelite is different from that of Example 1 only in that:
[0064] The pH value of the scheelite slurry in step (3) is 9.0;
[0065] In step (4), based on the weight of the original ore, the amount of inhibitor added during the roughing process is 80 g / t, and the amount of collector added is 300 g / t;
[0066] The amount of inhibitor added during the concentration process is 40g / t;
[0067] The amount of collector added during the scavenging process is 150g / t.
[0068] The other process steps and parameters are the same as those in Example 2.
[0069] Example 7
[0070] The application of sulfodisuccinic acid, a calcium-containing gangue inhibitor, in the flotation of scheelite is different from that of Example 1 only in that:
[0071] The pH value of the scheelite slurry in step (3) is 9.0;
[0072] In step (4), based on the weight of the original ore, the amount of inhibitor added during the roughing process is 80 g / t, and the amount of collector added is 400 g / t;
[0073] The amount of inhibitor added during the concentration process is 40g / t;
[0074] The amount of collector added during the scavenging process is 200g / t.
[0075] The other process steps and parameters are the same as those in Example 2.
[0076] Comparative Example 1
[0077] A scheelite flotation method, which differs from Example 6 only in that thiodisuccinic acid is replaced by water glass as a depressant, wherein the amount of water glass added in the roughing process is 500 g / t, and the amount of water glass added in the fine process is 250 g / t, based on the weight of the original ore. The other process steps and parameters are the same as those in Example 6.
[0078] Technical effect:
[0079] Table 1 shows the test results of WO3 grade in tungsten concentrate and tungsten recovery rate in tungsten concentrate obtained in Examples 1 to 7 and Comparative Example 1.
[0080] Among them, the calculation method of WO3 grade is:
[0081] The calculation method of tungsten recovery rate is:
[0082] Where, ξ is the tungsten recovery rate in concentrate, %; m 精 、m 原 are the mass of concentrate and ore, g; α 精 , α 原 They are the WO3 grades in concentrate and ore respectively.
[0083] Table 1 Experimental conditions of Examples 1-7 and Comparative Examples 1-3 and test results of tungsten concentrate grade and recovery rate
[0084] Sample <![CDATA[WO3 grade (%)]]> Tungsten recovery rate (%) Example 1 54.16 84.63 Example 2 56.07 86.22 Example 3 55.21 85.34 Example 4 58.32 82.19 Example 5 61.07 79.38 Example 6 59.25 84.71 Example 7 57.98 86.85 Comparative Example 1 49.36 76.58
[0085] It can be seen from the results of Example 6 and Comparative Example 1 that when the inhibitor thiodisuccinic acid of the present invention is used to sort a certain scheelite, better mineral processing indicators can be obtained at a lower dosage. The WO3 grade in the tungsten concentrate is 9.89% higher than that of the conventional inhibitor water glass, and the tungsten recovery rate is 8.13% higher, which is much better than the sorting indicators when water glass is used as a inhibitor.
[0086] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. Application of sulfodisuccinic acid, a calcium-containing gangue inhibitor, in the flotation of scheelite.
2. A method for flotation of scheelite, comprising crushing, grinding, slurry preparation and flotation, characterized in that: In the flotation process, sulfodisuccinic acid is used as an inhibitor and sodium oleate is used as a collector.
3. The method for flotation of scheelite according to claim 2, characterized in that: The flotation process includes one roughing process, two cleaning processes and one scavenging process.
4. The method for flotation of scheelite according to claim 3, characterized in that: Sulfosuccinic acid and sodium oleate are added during the roughing process. Based on the mass of the original ore, the added amount of sulfosuccinic acid is 60-100 g / t, and the added amount of sodium oleate is 200-400 g / t.
5. The method for flotation of scheelite according to claim 3, characterized in that: Supplementary sulfodisuccinic acid is added during the beneficiation process. Based on the mass of the original ore, the amount of the supplementary sulfodisuccinic acid is 30 to 50 g / t.
6. The method for flotation of scheelite according to claim 3, characterized in that: Sodium oleate is added during the scavenging process. Based on the mass of the original ore, the added amount of sodium oleate is 100-200 g / t.
7. A scheelite flotation method according to any one of claims 2 to 6, characterized in that: The sulfosuccinic acid and sodium oleate are both added in the form of solutions; Wherein, the mass concentration of thiodisuccinic acid solution is 1%; The mass concentration of the sodium oleate solution is 1%.
8. The method for flotation of scheelite according to claim 2, characterized in that: The slurry preparation is to mix the scheelite powder obtained after grinding with an alkaline solution and water to prepare scheelite slurry.
9. The method for flotation of scheelite according to claim 8, characterized in that: The alkaline solution is a sodium carbonate solution or a sodium bicarbonate solution with a mass concentration of 1%.
10. The method for flotation of scheelite according to claim 8, characterized in that: In the scheelite slurry, the mass concentration of scheelite is 15-30%, and the pH value is 7.0-10.5.
Citation Information
Cited By
Collecting agent and method for flotation of non-sulfide ore
CN120115297A