Rolling method for controlling structure uniformity of plain round steel bars
By controlling the rolling process of steel bars, including heating, rolling and cooling steps, the problems of unstable steel bar performance and uneven structure in the prior art are solved, and the uniformity and high-quality production of steel bars are achieved. The process is simple and not New equipment is required.
Patent Information
- Application Number
- CN202411030059.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-30
AI Technical Summary
There are problems of unstable performance and uneven structure in the existing steel bar rolling technology, which affects the quality of steel bars.
Through a series of steps, including uniform heating, rough rolling, medium rolling, pre-finishing rolling, water cooling, finishing rolling, silk spinning and cooling, the tissue uniformity of the light round steel bars is controlled. The specific steps include heating the raw material to 1100-1115℃. Coarse rolling, medium rolling and pre-finishing rolling were carried out, water cooled to 850-860℃ for finishing rolling, and then heated to 930-940℃ for wire spinning. Finally, the light round steel bars were obtained by cooling through Steyrmo air-cooled rollers.
The uniformity of steel bar structure and stability of performance are achieved. The surface of the steel bar produced is smooth, with high quality, and does not require new equipment investment. The process is simple and suitable for widespread promotion.
Smart Images

Figure CN118875014A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel metallurgy rolling, and more specifically, to a rolling method for controlling the uniformity of the structure of smooth round steel bars. Background Art
[0002] Wire rods are a common form of steel materials. The uses of wire rods can be divided into two categories: one is to use wire rod products directly, mainly in reinforced concrete reinforcement and welded structural parts. The other is to use wire rods as raw materials after reprocessing. For example, rivets can be made through hot forging or cold forging, bolts can be made through cold forging and rolling, and machine parts or tools can be made through various cutting processes and heat treatments. Wire rods are not only widely used, but also used in large quantities, and they occupy a relatively important position in the national economy.
[0003] However, the existing technology for rolling steel bars is prone to unstable performance, uneven organization and other problems. Therefore, it is necessary to study a rolling method for controlling the uniformity of the smooth round steel bar organization to address the shortcomings of the existing technology, solve the problems of unstable steel bar performance and improve the quality of steel bars. Summary of the invention
[0004] The technical problem to be solved by the present invention is to address the above-mentioned deficiencies in the prior art, and an object of the present invention is to provide a rolling method for controlling the uniformity of the structure of round steel bars, which can improve the quality of steel bars.
[0005] The technical solution of the present invention is: a rolling method for controlling the uniformity of the structure of smooth round steel bars, comprising the following steps:
[0006] Step S1. uniformly heating the first raw material to a first temperature;
[0007] Step S2. maintaining the first raw material at the first temperature and sequentially performing rough rolling, intermediate rolling and pre-finishing rolling to obtain a second raw material;
[0008] Step S3. Cooling the second raw material to a second temperature with water, and then finishing rolling the second raw material to obtain a third raw material;
[0009] Step S4. heating the third raw material to a third temperature, and then spinning the third raw material to obtain a fourth raw material;
[0010] Step S5. After the spinning process, the fourth raw material is cooled to obtain a smooth round steel bar.
[0011] As a further improvement, the composition of the first raw material in step S1 is: C≤0.25, Si≤0.55, Mn≤1.50, P≤0.045, S≤0.045.
[0012] Furthermore, the first temperature in step S2 is 1100-1115° C., the rough rolling speed is 1-1.5 m / s, the intermediate rolling speed is 4-4.5 m / s, and the pre-finishing rolling speed is 9-9.5 m / s.
[0013] Furthermore, in step S2, the first temperature is 1108° C., the rough rolling speed is 1.2 m / s, the intermediate rolling speed is 4.2 m / s, and the pre-finishing rolling speed is 9.2 m / s.
[0014] Furthermore, the second temperature in step S3 is 850-860° C., and the finishing speed is 80-85 m / s.
[0015] Furthermore, the second temperature in step S3 is 855° C., and the finishing speed is 82 m / s.
[0016] Furthermore, the third temperature in step S4 is 930-940°C.
[0017] Furthermore, the third temperature in step S4 is 935°C.
[0018] Furthermore, in step S5, cooling is performed by a Stelmor air-cooled roller, with a total of 12 cooling roller passes and a roller speed of 0.5-0.7 m / s.
[0019] Furthermore, before rough rolling, intermediate rolling and pre-finishing rolling, the first raw material is subjected to heat preservation treatment, and the heat preservation treatment is performed by flame heating or high-frequency heating.
[0020] Beneficial Effects
[0021] Compared with the prior art, the present invention has the following advantages:
[0022] The steel bars produced by the method of the present invention have uniform structure, smooth surface, stable performance and high steel bar quality. The method of the present invention does not require investment in new equipment, has a simple process and is suitable for wide promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is a flow chart of the present invention;
[0024] Figure 2 The whole process flow chart of the production of round steel bars;
[0025] Figure 3 This is the process flow chart for rolling of round steel bars;
[0026] Figure 4 The metallographic diagram of the rolled sample of the prior art;
[0027] Figure 5 This is a metallographic diagram of the sample rolled by the method of the present invention. DETAILED DESCRIPTION
[0028] The present invention will be further described below with reference to the specific embodiments in the accompanying drawings.
[0029] See also Figure 1 to Figure 5 A rolling method for controlling the uniformity of the structure of a round steel bar comprises the following steps:
[0030] Step S1. uniformly heating the first raw material to a first temperature;
[0031] Step S2. maintaining the first raw material at the first temperature and sequentially performing rough rolling, intermediate rolling and pre-finishing rolling to obtain a second raw material;
[0032] Step S3. Cooling the second raw material to a second temperature with water, and then finishing rolling the second raw material to obtain a third raw material;
[0033] Step S4. heating the third raw material to a third temperature, and then spinning the third raw material to obtain a fourth raw material;
[0034] Step S5. After the spinning process, the fourth raw material is cooled to obtain a smooth round steel bar.
[0035] The entire process flow chart of round steel bar production is as follows Figure 2 As shown, the billet continuous casting machine A produces the billet B, and the billet B is cut to obtain the first raw material, which is transported to the heating furnace D through the roller trolley C. The heating furnace D evenly heats the first raw material to a first temperature, and then keeps the first temperature and sequentially passes through the roughing mill E, the steel dividing roller F, the intermediate rolling mill G, and the pre-finishing mill H for roughing, intermediate rolling and pre-finishing rolling to obtain the second raw material, the second raw material is water-cooled to the second temperature, and then the second raw material is input into the finishing mill I to obtain the third raw material, the third raw material is heated to the third temperature, and then the third raw material is input into the spinning machine J to obtain the fourth raw material, the fourth raw material is input into the cooling roller K for cooling to obtain the plain round steel bars, and the plain round steel bars are transported to the bundling station L for bundling and then put into storage.
[0036] Specifically, the composition of the first raw material in step S1 is: C≤0.25, Si≤0.55, Mn≤1.50, P≤0.045, S≤0.045.
[0037] The first temperature in step S2 is 1100-1115°C, the rough rolling speed is 1-1.5 m / s, the intermediate rolling speed is 4-4.5 m / s, and the pre-finishing rolling speed is 9-9.5 m / s. Preferably, the first temperature in step S2 is 1108°C, the rough rolling speed is 1.2 m / s, the intermediate rolling speed is 4.2 m / s, and the pre-finishing rolling speed is 9.2 m / s.
[0038] The second temperature in step S3 is 850-860°C, and the finishing speed is 80-85 m / s. Preferably, the second temperature in step S3 is 855°C, and the finishing speed is 82 m / s.
[0039] The third temperature in step S4 is 930-940° C. Preferably, the third temperature in step S4 is 935° C.
[0040] In step S5, cooling is performed by Stelmor air-cooled rollers, with a total of 12 cooling rollers, and the roller speed is 0.5-0.7 m / s. Preferably, the roller speed is 0.6 m / s.
[0041] Before rough rolling, intermediate rolling and pre-finishing rolling, the first raw material is subjected to heat preservation treatment. An infrared temperature detector is arranged above the conveying roller to detect the temperature of the first raw material in real time. The heat preservation treatment is performed by flame heating or high frequency heating.
[0042] A heating MAP table can be prepared in advance based on temperature and gas injection amount, that is, different temperatures of the first raw material correspond to different gas injection amounts, or a heating MAP table can be prepared based on temperature and high-frequency parameters, that is, different temperatures of the first raw material correspond to different high-frequency parameters, and the heating MAP table can be queried according to the actual temperature detected by the infrared temperature detector to obtain the target gas injection amount or the target high-frequency parameters, so as to control the operation of the spray gun according to the target gas injection amount, or control the operation of the high-frequency heater according to the target high-frequency parameters, so that the first raw material maintains the first temperature.
[0043] Practical Application:
[0044] The billet (first raw material) passes through a soaking section at 1100-1115°C, a rough rolling speed of 1.38m / s, an intermediate rolling speed of 4.15m / s, a pre-finishing rolling speed of 9.4m / s, and then is water-cooled to 850-860°C for finishing rolling, a finishing rolling speed of 82m / s, and then heated to 930-940°C for wire laying. Finally, the Stelmor air-cooled roller is cooled, with a total of 12 cooling rollers, and a roller speed of 0.5-0.7m / s. The specific implementation speed is shown in the following table.
[0045]
[0046] like Figure 4 The figure shows the random sampling before the rolling process of the prior art, and the random sampling after the rolling process of the present invention. Figure 5 As shown, it can be seen from the metallographic results that the sample has a uniform structure.
[0047] The above are only preferred embodiments of the present invention. It should be pointed out that for those skilled in the art, several modifications and improvements can be made without departing from the structure of the present invention, which will not affect the effect of the implementation of the present invention and the practicality of the patent.
Claims
1. A rolling method for controlling the uniformity of the structure of round steel bars, characterized in that: The following steps are involved: Step S1. uniformly heating the first raw material to a first temperature; Step S2. maintaining the first raw material at the first temperature and sequentially performing rough rolling, intermediate rolling and pre-finishing rolling to obtain a second raw material; Step S3. Cooling the second raw material to a second temperature with water, and then finishing rolling the second raw material to obtain a third raw material; Step S4. heating the third raw material to a third temperature, and then spinning the third raw material to obtain a fourth raw material; Step S5. After the spinning process, the fourth raw material is cooled to obtain a smooth round steel bar.
2. A rolling method for controlling the uniformity of the structure of a plain round steel bar according to claim 1, characterized in that: The composition of the first raw material in step S1 is: C≤0.25, Si≤0.55, Mn≤1.50, P≤0.045, S≤0.
045.
3. A rolling method for controlling the uniformity of the structure of a plain round steel bar according to claim 1, characterized in that: The first temperature in step S2 is 1100-1115° C., the rough rolling speed is 1-1.5 m / s, the intermediate rolling speed is 4-4.5 m / s, and the pre-finishing rolling speed is 9-9.5 m / s.
4. A rolling method for controlling the uniformity of the smooth round steel bar structure according to claim 3, characterized in that: The first temperature in step S2 is 1108° C., the rough rolling speed is 1.2 m / s, the intermediate rolling speed is 4.2 m / s, and the pre-finishing rolling speed is 9.2 m / s.
5. A rolling method for controlling the uniformity of the structure of round steel bars according to claim 1, characterized in that: The second temperature in step S3 is 850-860° C., and the finishing speed is 80-85 m / s.
6. A rolling method for controlling the uniformity of the structure of a plain round steel bar according to claim 5, characterized in that: The second temperature in step S3 is 855° C., and the finishing speed is 82 m / s.
7. A rolling method for controlling the uniformity of the structure of round steel bars according to claim 1, characterized in that: The third temperature in step S4 is 930-940°C.
8. A rolling method for controlling the uniformity of the structure of round steel bars according to claim 7, characterized in that: The third temperature in step S4 is 935°C.
9. A rolling method for controlling the uniformity of the structure of a plain round steel bar according to claim 1, characterized in that: In step S5, cooling is performed by a Stelmor air-cooled roller conveyor, with a total of 12 cooling roller conveyors and a roller conveyor speed of 0.5-0.7 m / s.
10. A rolling method for controlling the uniformity of the structure of a plain round steel bar according to claim 1, characterized in that: Before rough rolling, intermediate rolling and pre-finishing rolling, the first raw material is subjected to heat preservation treatment, wherein the heat preservation treatment is performed by flame heating or high-frequency heating.
Citation Information
Patent Citations
Control method of high speed wire bar hot rolling surface red rust
CN101108396A
High speed production method for controlling banded structure of low carbon steel wire rod
CN102671938A
Production process of high-carbon steel wire rod
CN111530923A
Medium-high carbon steel hot-rolled wire rod and production method thereof
CN111872113A
Control method for oxidized scale on surface of hot-rolled wire rod and hot-rolled wire rod
CN116475237A