Forging process of aluminum alloy runner plate

Through high-precision material analysis and automation technology, the aluminum alloy runner plate is heated and forged three times at a time, solving the problems of complex process and low efficiency in the existing technology, significantly improving production efficiency and material utilization, and meeting the convection of new energy vehicles High performance requirements for tray board materials.

CN118926846APending Publication Date: 2024-11-12SUZHOU BEIJIALI MASCH TECH CO LTD

Patent Information

Application Number
CN202411269584.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing aluminum alloy runner plate forging process is complex, and multiple heating and multiple forgings lead to inefficiency and low material utilization.

Method used

Using high-precision material analysis, automatic cutting, continuous heating, multiple forging and fine edge cutting treatment, combined with T6 heat treatment, ensure that the material is heated and forged three times at an appropriate temperature, and improves the density of the material by precisely controlling the temperature and time. and performance.

Benefits of technology

It greatly improves production efficiency and material utilization, achieves higher refined molding and material performance, and reduces costs and production time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926846A_ABST
    Figure CN118926846A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of forging, and discloses a forging process of an aluminum alloy runner plate, which comprises the following steps of: analyzing the aluminum alloy runner plate by adopting a material analyzer, cutting off a round-bar-shaped aluminum alloy runner plate material by adopting an automatic cutting-off machine, putting the cut-off material into a continuous heating furnace for heating, the 3150T forging machine 1 # equipment is used for pre-forging, the 3150T forging machine 2 # equipment is used for intermediate forging and final forging, the 500T edge trimmer is used for cutting off flash and burr residues, the T6 automatic heat treatment line is used for carrying out heat treatment on materials, the equipment is cleaned, the fluorescent flaw detection line is used for carrying out fluorescent flaw detection on the materials, and the packaging station is checked. According to the forging process of the aluminum alloy runner plate, through one-time heating and three-time forging forming of the round bar, compared with an existing process of two-time heating and four-time forging, the efficiency is higher, the great process difficulty is broken through, the production efficiency and the material utilization rate are greatly improved, the subversive advanced process is achieved in the runner plate forging field, and the cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of forging, in particular to a forging process for an aluminum alloy flow channel plate. Background Art

[0002] The flow plate is an important component of the heat exchange management system in new energy vehicles. For new energy vehicles, especially electric vehicles and hybrid vehicles, the thermal management system is crucial to ensure vehicle performance, improve energy efficiency and extend battery life. The heat exchange management system is mainly responsible for regulating and maintaining the temperature of key components inside the vehicle (such as battery packs, motors, controllers, etc.) within an appropriate range. As a core component in the heat exchange management system, the design and function of the flow plate directly affect the efficiency and effect of heat exchange. It is usually located inside the heat exchanger and guides the flow of cooling media (such as coolant, refrigerant or air) through a specific flow channel design to achieve effective transfer and dissipation of heat.

[0003] The larger flow channel plate is heated for the first time, then preformed for the first time by forging, preformed for the second time by forging, heated for the second time, preformed for the third time by forging, and finally formed by forging for the fourth time. The process is relatively complicated, with two heatings and four forgings, which is extremely inefficient and has low material utilization. Therefore, it is necessary to design a corresponding technical solution to solve the problem. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In view of the deficiencies in the prior art, the present invention provides a forging process for an aluminum alloy runner plate, which solves the technical problems of complex process, multiple heating and multiple forging, extremely low efficiency and low material utilization.

[0006] (II) Technical solution

[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions: a forging process of an aluminum alloy flow channel plate, the method steps include the following:

[0008] S1. Material storage: Before the purchased aluminum alloy runner plate raw materials are stored, a high-precision material analyzer is used to conduct detailed chemical composition, physical properties and microstructure analysis to ensure that the materials meet the standards required by the forging process, laying a solid foundation for subsequent processing;

[0009] S2. Material cutting: Use an automatic cutting machine to accurately cut the round rod type aluminum alloy runner plate material according to the preset size specifications to ensure that the length and cross-section quality of each section of material meet the process requirements;

[0010] S3. Material heating: The cut aluminum alloy material is smoothly fed into the continuous heating furnace. Through the precisely controlled heating curve, the temperature inside and outside the material is ensured to be uniform and reach the temperature range suitable for forging.

[0011] S4, Pre-forging: Use 3150T forging machine-1# equipment to pre-forge the heated aluminum alloy material. Through reasonable die design and forging force control, the basic outline and size of the runner plate are preliminarily formed to prepare for subsequent fine forging;

[0012] S5, intermediate forging + final forging: On the 3150T forging machine-2# equipment, after further refinement and shaping by intermediate forging, combined with precise shaping by final forging, multiple pressing and corrections are performed to ensure that the shape, size and internal structure of the aluminum alloy runner plate meet the design requirements, while improving the density and mechanical properties of the material;

[0013] S6. Trimming: Use a 500T trimming machine to perform fine trimming on the forged runner plate to completely remove the flash and burr residues;

[0014] After pickling, visual inspection is performed to ensure that the material surface is free of oil, impurities and severe burrs;

[0015] Use 3D scanners to perform high-precision inspections on the flatness of materials to ensure that the flatness of products meets the standards;

[0016] S7, T6 heat treatment: The forged aluminum alloy runner plate is sent to the T6 automatic heat treatment line for solution treatment and aging treatment. By precisely controlling the temperature and time, the internal structure of the material reaches the optimal state, significantly improving the strength, hardness and corrosion resistance of the material while maintaining good toughness;

[0017] S8, cleaning: Place the heat-treated flow channel plate in a high-efficiency cleaning device and use an environmentally friendly cleaning agent to thoroughly remove surface residues to ensure a smooth surface of the material;

[0018] Further surface treatment, including sandblasting and anodizing, is performed when necessary;

[0019] S9, Fluorescent flaw detection: On the fluorescent flaw detection line, the aluminum alloy runner plate is fully inspected using fluorescent penetrants. Through ultraviolet irradiation, the defects of cracks and pores inside the material are visually displayed and evaluated to ensure that the product has no internal defects and meets high quality requirements;

[0020] S10. Shipping inspection and packaging: Before shipping, each aluminum alloy runner plate is carefully inspected for appearance, size and performance to ensure that all products meet the order requirements and industry standards;

[0021] Subsequently, the products are properly packaged using special packaging materials and methods to prevent damage during transportation, and are attached with complete product identification and inspection reports in preparation for shipment.

[0022] Preferably, in step S1, the raw materials of the aluminum alloy flow channel plate include Al, Fe, Si, Cu, Mg, Mn, Zn, Cr and Ti, wherein the proportion is: the balance is Al, the Fe proportion is set to ≤0.35%, the Si proportion is set to 0.2-0.6%, the Cu proportion is set to ≤0.1%, the Mg proportion is set to 0.45-0.9%, the Mn proportion is set to ≤0.1%, the Zn proportion is set to ≤0.1%, the Cr proportion is set to ≤0.1%, and the Ti proportion is set to ≤0.1%.

[0023] Preferably, the raw materials of the aluminum alloy flow channel plate are formulated in proportion: the balance is Al, the Fe proportion is set to 0.276%, the Si proportion is set to 0.563%, the Cu proportion is set to 0.0084%, the Mg proportion is set to 0.607%, the Mn proportion is set to ≤0.0609%, the Zn proportion is set to 0.0065%, the Cr proportion is set to 0.0835%, and the Ti proportion is set to 0.0824%.

[0024] Preferably, in step S3, the furnace temperature is set to 480-530°C and measured by a temperature regulator; the material surface temperature is 440-480°C and measured by a contact thermometer; and the material is in the furnace for 40 min to 180 min.

[0025] Preferably, in steps S4 and S5, the mold temperature is maintained at 200° C. to 300° C., and the mold size is 4-18±0.5 mm.

[0026] Preferably, in step S2, the cutting size is 275±1.0 mm and the diameter is φ95±0.5 mm.

[0027] Preferably, in step S7, the solution treatment temperature is 450-550°C, the solution treatment holding time is 40-80min, the quenching water temperature is 25-40°C, the quenching delay is ≤25s, the immersion time is ≥5min, the aging treatment temperature is 150-200°C, the aging treatment holding time is 120-180min, and the hardness is ≥HB70.

[0028] (III) Beneficial effects

[0029] Compared with the prior art, the invention has the following beneficial effects: by heating the round bar once and forging it three times, it breaks through the great process difficulty, greatly improves the production efficiency and material utilization rate, and realizes a subversive advanced process in the field of runner plate forging;

[0030] The split method was selected during the mold design process, which makes installation easier and reduces costs;

[0031] Compared with the plate raw materials of the existing process, the present invention uses round bars, which is low in cost and the weight of the entire mold product is reduced to 1 kg;

[0032] The material utilization rate of the present invention is more than 70% compared with 50-60% in the existing process;

[0033] The present invention heats once and performs forging three times, which is more efficient than the prior art of heating twice and performing forging four times.

[0034] The present invention is a refined molding process, wherein the hole depth and flow channel depth are twice as large as those of the existing process;

[0035] The time for the later fine processing of the present invention is 30 minutes, while the existing process takes 1-2 hours;

[0036] The process production line of the present invention is controlled by a robot arm throughout the entire process, does not require manual operation, adopts two forging main machines and two heating furnaces for operation, and has high efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is a schematic diagram of the simplified forging steps of the present invention;

[0038] Figure 2 It is a schematic diagram of pre-forging of the present invention;

[0039] Figure 3 It is a schematic diagram of the pre-forging lower die of the present invention;

[0040] Figure 4 It is a schematic diagram of the pre-forging upper die of the present invention;

[0041] Figure 5 It is a schematic diagram of the intermediate forging of the present invention;

[0042] Figure 6 It is a schematic diagram of the intermediate forging lower die of the present invention;

[0043] Figure 7 It is a schematic diagram of the intermediate forging upper die of the present invention;

[0044] Figure 8 It is a schematic diagram of final forging of the present invention;

[0045] Fig. 9 It is a schematic diagram of the final forging lower die of the present invention;

[0046] Fig.10 It is a schematic diagram of the final forging upper die of the present invention;

[0047] Fig.11 It is a schematic diagram of the layout of the flow channel plate production line of the present invention. DETAILED DESCRIPTION

[0048] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] See also Figure 1-Figure 11 The embodiment of the present invention provides a technical solution: a forging process of an aluminum alloy runner plate, the method steps include the following:

[0050] S1. Material storage: Before the purchased aluminum alloy runner plate raw materials are stored, a high-precision material analyzer is used to conduct detailed chemical composition, physical properties and microstructure analysis to ensure that the materials meet the standards required by the forging process, laying a solid foundation for subsequent processing;

[0051] S2. Material cutting: Use an automatic cutting machine to accurately cut the round rod type aluminum alloy runner plate material according to the preset size specifications to ensure that the length and cross-sectional quality of each section of material meet the process requirements, reduce material waste and improve production efficiency;

[0052] S3. Material heating: The cut aluminum alloy material is smoothly fed into the continuous heating furnace. Through the precisely controlled heating curve, the temperature inside and outside the material is ensured to be uniform and reach the temperature range suitable for forging, which can avoid coarse grains caused by overheating and prevent the forging effect from being affected by insufficient temperature.

[0053] S4, Pre-forging: Use 3150T forging machine-1# equipment to pre-forge the heated aluminum alloy material. Through reasonable die design and forging force control, the basic outline and size of the runner plate are preliminarily formed to prepare for subsequent fine forging;

[0054] S5, intermediate forging + final forging: On the 3150T forging machine-2# equipment, after further refinement and shaping by intermediate forging, combined with precise shaping by final forging, multiple pressing and corrections are performed to ensure that the shape, size and internal structure of the aluminum alloy runner plate meet the design requirements, while improving the density and mechanical properties of the material;

[0055] S6. Trimming: Use a 500T trimming machine to perform fine trimming on the forged runner plate to completely remove the flash and burr residues;

[0056] After pickling, visual inspection is performed to ensure that the material surface is free of oil, impurities and severe burrs;

[0057] Use 3D scanners to perform high-precision inspections on the flatness of materials to ensure that the flatness of products meets the standards;

[0058] S7, T6 heat treatment: The forged aluminum alloy runner plate is sent to the T6 automatic heat treatment line for solution treatment and aging treatment. By precisely controlling the temperature and time, the internal structure of the material reaches the optimal state, significantly improving the strength, hardness and corrosion resistance of the material while maintaining good toughness;

[0059] S8, cleaning: Place the heat-treated flow channel plate in a high-efficiency cleaning device and use an environmentally friendly cleaning agent to thoroughly remove surface residues to ensure a smooth surface of the material;

[0060] Further surface treatment, including sandblasting and anodizing, is performed when necessary to enhance the material's appearance and weather resistance;

[0061] S9, Fluorescent flaw detection: On the fluorescent flaw detection line, the aluminum alloy runner plate is fully inspected using fluorescent penetrants. Through ultraviolet irradiation, the defects of cracks and pores inside the material are visually displayed and evaluated to ensure that the product has no internal defects and meets high quality requirements;

[0062] S10. Shipping inspection and packaging: Before shipping, each aluminum alloy runner plate is carefully inspected for appearance, size and performance to ensure that all products meet the order requirements and industry standards;

[0063] Subsequently, the products are properly packaged using special packaging materials and methods to prevent damage during transportation, and are attached with complete product identification and inspection reports in preparation for shipment.

[0064] Further improved, in step S1, the raw materials of the aluminum alloy flow channel plate include Al, Fe, Si, Cu, Mg, Mn, Zn, Cr and Ti, wherein the proportion is: the balance is Al, the Fe proportion is set to ≤0.35%, the Si proportion is set to 0.2-0.6%, the Cu proportion is set to ≤0.1%, the Mg proportion is set to 0.45-0.9%, the Mn proportion is set to ≤0.1%, the Zn proportion is set to ≤0.1%, the Cr proportion is set to ≤0.1%, and the Ti proportion is set to ≤0.1%.

[0065] Further improved, the raw materials of the aluminum alloy flow channel plate are prepared in proportion: the balance is Al, the Fe ratio is set to 0.276%, the Si ratio is set to 0.563%, the Cu ratio is set to 0.0084%, the Mg ratio is set to 0.607%, the Mn ratio is set to ≤0.0609%, the Zn ratio is set to 0.0065%, the Cr ratio is set to 0.0835%, and the Ti ratio is set to 0.0824%;

[0066] It ensures that the aluminum alloy runner plate has excellent mechanical properties, corrosion resistance and machinability. The addition of Mg improves the strength and corrosion resistance of the alloy, while an appropriate amount of Si helps to improve the casting performance and fluidity of the alloy; the content of trace elements such as Mn, Zn, and Cu is strictly controlled to avoid the adverse effects of impurity elements on alloy properties and ensure the high purity and consistency of the aluminum alloy runner plate; the reasonable element ratio not only improves the strength, hardness and wear resistance of the alloy, but also maintains good toughness and plasticity, meeting the high requirements of the heat exchange management system of new energy vehicles for runner plate materials.

[0067] Further improved, in step S3, the furnace temperature is set to 480-530°C, measured by a temperature regulator; the material surface temperature is 440-480°C, measured by a contact thermometer; the material is in the furnace for 40min to 180min;

[0068] By setting a reasonable furnace temperature and using a temperature regulator and contact thermometer for precise measurement, the material is ensured to be heated evenly during the heating process, avoiding performance degradation and defects caused by overheating or overcooling; the optimized furnace time ensures that the material fully reaches the temperature required for forging, while avoiding grain growth and structural coarsening that may be caused by heating for too long.

[0069] Further improved, in steps S4 and S5, the mold temperature is maintained at 200°C to 300°C, and the mold size is 4-18±0.5mm;

[0070] Keeping the temperature between 200℃ and 300℃ helps to reduce thermal stress during forging, improve die life, and promote good flow and forming of materials; strictly controlling the die size and its tolerance ensures that the forged runner plate has precise size and shape to meet design requirements.

[0071] As a further improvement, in step S2, the cutting size is 275±1.0 mm and the diameter is φ95±0.5 mm. This high-precision cutting ensures the stability and consistency of the material in the subsequent forging process and reduces waste and errors in the processing process.

[0072] Specifically, in step S7, the solution treatment temperature is 450-550°C, the solution treatment holding time is 40-80min, the quenching water temperature is 25-40°C, the quenching delay is ≤25s, the immersion time is ≥5min, the aging treatment temperature is 150-200°C, the aging treatment holding time is 120-180min, and the hardness is ≥HB70;

[0073] By precisely controlling the solution treatment temperature, time, quenching water temperature, quenching delay and immersion time, the aluminum alloy runner plate is ensured to obtain the ideal microstructure and performance during the heat treatment process; the optimized aging treatment temperature and time further improve the hardness and strength of the alloy while maintaining good toughness, meeting the strict requirements of new energy vehicles for material properties.

[0074] It not only improves the overall performance of the aluminum alloy runner plate, but also improves production efficiency and product quality, reduces production costs, and is of great significance to the development of the new energy vehicle industry.

[0075] In summary, by heating the round bar once and forging it three times, we have overcome great process difficulties, greatly improved production efficiency and material utilization, and realized a disruptive advanced process in the field of runner plate forging.

[0076] Aluminum alloys need to be heated before hot forging to reach a suitable forging temperature; the heating temperature is between 400℃ and 550℃, and the temperature is set according to the specific type and shape of the aluminum alloy. Too high or too low a temperature will affect the forging quality of the aluminum alloy. During the heating process, the heating speed should be controlled to avoid heat loss or overheating caused by too fast or too slow heating;

[0077] The forging of aluminum alloy is to place the aluminum billet in a forging die and use external force to make it plastically deform to achieve the required shape and size. The force and forging speed are controlled during the forging process to avoid excessive deformation or insufficient forging. At the same time, attention should be paid to maintaining a sufficient forging temperature so that the aluminum alloy does not produce cracks and defects when deformed.

[0078] The split method was selected during the mold design process, which makes installation easier and reduces costs;

[0079] Compared with the plate raw materials of the existing process, the present invention uses round bars, which is low in cost and the weight of the entire mold product is reduced to 1 kg;

[0080] The material utilization rate of the present invention is more than 70% compared with 50-60% in the existing process;

[0081] The present invention heats once and performs forging three times, which is more efficient than the prior art of heating twice and performing forging four times.

[0082] The present invention is a refined molding process, wherein the hole depth and flow channel depth are twice as large as those of the existing process;

[0083] The time for the later fine processing of the present invention is 30 minutes, while the existing process takes 1-2 hours;

[0084] The process production line of the present invention is controlled by a robot arm throughout the entire process, does not require manual operation, adopts two forging main machines and two heating furnaces for operation, and has high efficiency.

[0085] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. Any figure mark in the claims should not be regarded as limiting the claims involved.

[0086] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A forging process for an aluminum alloy runner plate, characterized in that: The method steps include the following: S1. Material storage: Before the purchased aluminum alloy runner plate raw materials are stored, a high-precision material analyzer is used to conduct detailed chemical composition, physical properties and microstructure analysis to ensure that the materials meet the standards required by the forging process, laying a solid foundation for subsequent processing; S2. Material cutting: Use an automatic cutting machine to accurately cut the round rod type aluminum alloy runner plate material according to the preset size specifications to ensure that the length and cross-section quality of each section of material meet the process requirements; S3. Material heating: The cut aluminum alloy material is smoothly fed into the continuous heating furnace. Through the precisely controlled heating curve, the temperature inside and outside the material is ensured to be uniform and reach the temperature range suitable for forging. S4, Pre-forging: Use 3150T forging machine-1# equipment to pre-forge the heated aluminum alloy material. Through reasonable die design and forging force control, the basic outline and size of the runner plate are preliminarily formed to prepare for subsequent fine forging; S5, intermediate forging + final forging: On the 3150T forging machine-2# equipment, after further refinement and shaping by intermediate forging, combined with precise shaping by final forging, multiple pressing and corrections are performed to ensure that the shape, size and internal structure of the aluminum alloy runner plate meet the design requirements, while improving the density and mechanical properties of the material; S6. Trimming: Use a 500T trimming machine to perform fine trimming on the forged runner plate to completely remove the flash and burr residues; After pickling, visual inspection is performed to ensure that the material surface is free of oil, impurities and severe burrs; Use 3D scanners to perform high-precision inspections on the flatness of materials to ensure that the flatness of products meets the standards; S7, T6 heat treatment: The forged aluminum alloy runner plate is sent to the T6 automatic heat treatment line for solution treatment and aging treatment. By precisely controlling the temperature and time, the internal structure of the material reaches the optimal state, significantly improving the strength, hardness and corrosion resistance of the material while maintaining good toughness; S8, cleaning: Place the heat-treated flow channel plate in a high-efficiency cleaning device and use an environmentally friendly cleaning agent to thoroughly remove surface residues to ensure a smooth surface of the material; Further surface treatment, including sandblasting and anodizing, is performed when necessary; S9, Fluorescent flaw detection: On the fluorescent flaw detection line, the aluminum alloy runner plate is fully inspected using fluorescent penetrants. Through ultraviolet irradiation, the defects of cracks and pores inside the material are visually displayed and evaluated to ensure that the product has no internal defects and meets high quality requirements; S10. Shipping inspection and packaging: Before shipping, each aluminum alloy runner plate is carefully inspected for appearance, size and performance to ensure that all products meet the order requirements and industry standards; Subsequently, the products are properly packaged using special packaging materials and methods to prevent damage during transportation, and are attached with complete product identification and inspection reports in preparation for shipment.

2. The forging process of an aluminum alloy runner plate according to claim 1, characterized in that: In step S1, the raw materials of the aluminum alloy flow channel plate include Al, Fe, Si, Cu, Mg, Mn, Zn, Cr and Ti, which are prepared in proportion as follows: the balance is Al, the Fe ratio is set to ≤0.35%, the Si ratio is set to 0.2-0.6%, the Cu ratio is set to ≤0.1%, the Mg ratio is set to 0.45-0.9%, the Mn ratio is set to ≤0.1%, the Zn ratio is set to ≤0.1%, the Cr ratio is set to ≤0.1%, and the Ti ratio is set to ≤0.1%.

3. The forging process of an aluminum alloy runner plate according to claim 2, characterized in that: The raw materials of the aluminum alloy flow channel plate are prepared in proportion: the balance is Al, the Fe ratio is set to 0.276%, the Si ratio is set to 0.563%, the Cu ratio is set to 0.0084%, the Mg ratio is set to 0.607%, the Mn ratio is set to ≤0.0609%, the Zn ratio is set to 0.0065%, the Cr ratio is set to 0.0835%, and the Ti ratio is set to 0.0824%.

4. The forging process of an aluminum alloy runner plate according to claim 1, characterized in that: In step S3, the furnace temperature is set to 480-530°C and measured by a temperature regulator; the material surface temperature is 440-480°C and measured by a contact thermometer; the material is in the furnace for 40min to 180min.

5. The forging process of an aluminum alloy runner plate according to claim 1, characterized in that: In steps S4 and S5, the mold temperature is maintained at 200°C to 300°C, and the mold size is 4-18±0.5mm.

6. The forging process of an aluminum alloy runner plate according to claim 1, characterized in that: In step S2, the cutting size is 275±1.0 mm and the diameter is φ95±0.5 mm.

7. The forging process of an aluminum alloy runner plate according to claim 1, characterized in that: In step S7, the solution treatment temperature is 450-550°C, the solution treatment holding time is 40-80min, the quenching water temperature is 25-40°C, the quenching delay is ≤25s, the immersion time is ≥5min, the aging treatment temperature is 150-200°C, the aging treatment holding time is 120-180min, and the hardness is ≥HB70.

Citation Information

Patent Citations

  • Production process of high-strength and high-toughness forged aluminum alloy wheel

    CN109604974A

  • Machining method of axial flow type compressor stator blade flow channel plate

    CN110076524A

  • Light high-yield-strength aluminum alloy hub and forging process thereof

    CN114196858A

  • Casting and forging process for aluminum alloy forge piece of new energy automobile

    CN116871446A

  • Curved surface split die forging method for T-shaped aluminum alloy die forging

    CN117564203A

Cited By

  • Aluminum alloy material forming process

    CN119457738A