Production process for direct casting of small square billet low-carbon cold forging steel
By controlling the parameters of the argon station and LF process in the low-carbon cold heading steel production process and optimizing the tundish treatment, the direct pouring of low-carbon cold heading steel in the billet is achieved, solving the problem of poor water-watering ability and reducing the problem of low-carbon cold heading steel in the molten steel. Production costs and improve success rates.
Patent Information
- Application Number
- CN202411201362.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-01
AI Technical Summary
The poor water-water castability of low-carbon cold heading steel leads to the need to use Q195 and HPB300 as head furnaces to pour continuously, increasing the processing volume of low-end wire drawing materials and general materials, affecting production efficiency.
Using the converter process-argon station process-LF process-billet continuous casting process, the Al content, temperature, Si content and Ca content in the molten steel are controlled, the baking temperature is controlled in the middle, and the argon blowing protection and covering agent are implemented. Stable control of pulling speed to achieve direct pouring of small square low-carbon cold heading steel.
The Q195 and HPB300 were abolished as head furnace continuous pouring, which reduced the processing volume of low-end wire drawing materials and general materials, reduced production costs, and improved the direct pouring success rate of low-carbon cold heading steel in billet continuous casting machines.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a production process for directly casting small square billet low-carbon cold heading steel. Background Art
[0002] Low-carbon cold-forging steel is widely used in the production of standard parts such as screws, pins, and nuts. The cold-forging process saves raw materials and reduces costs. It also increases the tensile strength of the workpiece through cold work hardening, improving performance.
[0003] Low-carbon cold-heading steel has poor castability. To address this, Q195 and HPB300 are typically used for continuous casting in the lead furnace. This increases the processing capacity of low-end wire drawing materials and general materials, seriously affecting the company's production efficiency and is undesirable for the pursuit of economical steelmaking. Therefore, it is necessary to directly cast low-carbon cold-heading steel from small billets. Summary of the Invention
[0004] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and to provide a production process for directly casting small square billet low-carbon cold heading steel.
[0005] The present invention solves the technical problem by adopting the following technical solutions.
[0006] An embodiment of the present invention provides a production process for direct casting of low-carbon cold heading steel for small square billets. The production process of low-carbon cold heading steel for small square billets includes: a converter process-an argon station process-an LF process-a small square billet continuous casting process. The Al content in the molten steel is controlled in the argon station process, the temperature, Al content, Si content and Ca content of the molten steel are controlled in the LF process, the baking temperature of the continuous casting tundish is controlled, argon blowing control is implemented in each link of the continuous casting, a covering agent is added to the tundish, and the casting speed is stably controlled, thereby ultimately achieving direct casting of low-carbon cold heading steel for small square billets.
[0007] The present invention has the following beneficial effects:
[0008] The present invention provides a production process for direct casting of low-carbon cold-heading steel in billets. By optimizing the argon station process, the LF process, and the billet continuous casting process, the process enables direct casting of low-carbon cold-heading steel in the billet continuous casting machine. This eliminates the need for Q195 and HPB300 as the first furnace for continuous casting, reduces the processing volume of low-end wire drawing materials and general materials, and lowers production costs. DETAILED DESCRIPTION
[0009] To make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are described clearly and completely below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer are used. Where the manufacturer of the reagents or instruments is not specified, all are conventional products that can be purchased commercially.
[0010] The following is a detailed description of a production process for direct casting of low-carbon cold heading steel billets provided in an embodiment of the present invention.
[0011] An embodiment of the present invention provides a production process for direct casting of low-carbon cold heading steel for small square billets. The production process of low-carbon cold heading steel for small square billets includes: a converter process-an argon station process-an LF process-a small square billet continuous casting process. The Al content in the molten steel is controlled in the argon station process, the temperature, Al content, Si content and Ca content of the molten steel are controlled in the LF process, the baking temperature of the continuous casting tundish is controlled, argon blowing control is implemented in each link of the continuous casting, a covering agent is added to the tundish, and the casting speed is stably controlled, thereby ultimately achieving direct casting of low-carbon cold heading steel for small square billets.
[0012] The controlled composition of low-carbon cold-heading steel is generally: C 0.08-0.20%, Al 0.30-0.50%, Cr≤0.05%, Si≤0.10%, Mn 0.30-0.60%, and certain trace elements. This series of steels, with their low C content and high Al content, has poor castability. During the first pour, Al2O3 nozzle nodules are easily formed due to oxidation of the molten steel, leading to pouring failure. After long-term practice and observation, the inventors have proposed a production process for direct pouring of low-carbon cold-heading steel in billets. By optimizing the argon station process, the LF process, and the billet continuous casting process, this allows direct pouring of low-carbon cold-heading steel in the billet continuous caster. This eliminates the need for Q195 and HPB300 steels for the first pour, reduces the processing volume of low-end wire drawing material and general materials, and lowers production costs.
[0013] In an optional embodiment, controlling the Al content in the molten steel in the argon station process includes: controlling the Al content in the molten steel in the argon station process to be 0.030-0.060%.
[0014] In an optional embodiment, controlling the Al content, Si content and Ca content in the molten steel in the LF process includes: first controlling the ladle clearance ≥300mm, and the ladle clearance includes the vertical bricks at the ladle mouth to reduce the molten steel spraying when feeding the calcium line, adding Al to 0.045-0.050% according to sample 1, and subsequently trying not to add aluminum, and adding Si to 0.065% according to sample 2.
[0015] In an optional embodiment, it also includes: after the molten steel is supplemented with aluminum and before feeding the calcium line, controlling the molten steel temperature to 1620°C and the Al content to 0.046%, then feeding the calcium line and performing soft blowing, so that the Ca content in the LF outgoing molten steel is 30-45ppm, the Al content is 0.031%, and the Si content is 0.07-0.09%.
[0016] The present invention provides a production process for direct casting of low-carbon cold-heading steel billets. During the LF process, by optimizing the Al control method for each steel grade, deoxidation of the molten steel is completed as soon as possible, allowing sufficient time for the deoxidation product, Al2O3, to float. The Si content in the molten steel is optimized to minimize the [O] content, thereby reducing Al2O3 formation. The Ca content in the molten steel is optimized, controlling the outgoing Ca content to 30-45 ppm. The higher Ca content in the molten steel reacts with Al2O3 to form the low-melting-point 12CaO7·Al2O3, thus preventing nozzle sprue formation.
[0017] In an optional embodiment, controlling the molten steel temperature during the LF process includes controlling the molten steel temperature at the LF exit to TL + 75°C and the molten steel temperature on the continuous casting platform to TL + 70°C, ensuring a tundish superheat of 37-45°C, where TL is the liquidus temperature of the molten steel. A higher superheat helps improve the fluidity of the molten steel and compensates for heat absorption by the refractory during the pouring process, thereby increasing the success rate of the pouring process.
[0018] In an optional embodiment, controlling the baking temperature of the continuous casting tundish includes controlling the baking temperature of the continuous casting tundish to 1200-1250°C and adding calcium wire to the tundish before pouring, with the amount added to the tundish near the flow baking hole being 10m3 and the amount added to the steel receiving port being 20m3. Adding calcium wire to the tundish further treats Ca in the molten steel, optimizes the pouring operation, and increases the success rate of the pouring.
[0019] In an optional embodiment, each step of implementing argon blowing control to reduce secondary oxidation of molten steel includes:
[0020] a. Before pouring, the tundish is moving, and argon is blown into the tundish body using an elbow argon blowing pipe at 1800L / min for more than 3 minutes;
[0021] b. The tundish is transported to the casting position, and the tundish is blown with argon at the steel mouth at 250L / min for more than 2 minutes;
[0022] c. Argon blowing of 150L / min at the ladle slide mechanism during the pouring process;
[0023] d. During the pouring process, the argon sealing ring of the ladle long nozzle is blown at 350L / min. This optimizes the protective pouring process, effectively reduces the oxidation of Al in the molten steel by the air during pouring, and reduces the secondary oxidation of the molten steel to form Al2O3 inclusions.
[0024] In an optional embodiment, adding a covering agent into the tundish includes: covering the molten steel in the tundish with an insulation method combining a magnesium covering agent and carbonized rice husks; when the weight of the molten steel in the first furnace reaches about 7 tons, 50 kg of magnesium covering agent is added to each baking hole in the non-impact zone; when the weight of the molten steel in the tundish reaches 18 tons, 100 kg of magnesium covering agent is added to the steel receiving port; and when the first furnace tundish is poured, no less than 400 kg of magnesium covering agent is added.
[0025] In an optional embodiment, it also includes: before the ladle starts pouring, the tundish stopper rod is pre-tested to ensure reliable operation of the mechanism.
[0026] In an optional embodiment, the stable control of the casting speed includes: all casting modes adopt a manual small steel flow steadily pressurized starting method, and the starting casting speed is uniformly set to 1.0m / min.
[0027] The present invention will be further described below with reference to the embodiments.
[0028] Example 1
[0029] A direct casting process for billet low-carbon cold-heading steel is described. The production process includes: converter process - argon station process - LF process - billet continuous casting process. The Al content in the molten steel is controlled in the argon station process, the temperature, Al content, Si content and Ca content of the molten steel are controlled in the LF process, the baking temperature of the continuous casting tundish is controlled, argon blowing is controlled in each step of the continuous casting process, a covering agent is added to the tundish, and the casting speed is stably controlled, ultimately achieving direct casting of billet low-carbon cold-heading steel. Specifically:
[0030] (1) The clearance of the ladle is 320mm (including the vertical brick of the ladle mouth) to reduce the spraying of molten steel when feeding the Ca wire.
[0031] (2) Control the Al content in the molten steel at the argon station to 0.055%.
[0032] (3) According to sample 1, add Al to 0.048%, and try not to add aluminum later. According to sample 2, add Si to 0.065%; before feeding the Ca line, control the Al content to about 0.046%, the temperature reference: 1620℃, control the outgoing Al content to about 0.031%, the Si content to 0.08%, and the Ca content to 35ppm (target 35-45ppm).
[0033] (4) The outlet temperature of molten steel in the LF process is TL+75℃, and the reference temperature of the continuous casting platform is TL+70℃ to ensure that the superheat of the tundish is between 37-45℃.
[0034] (5) The baking temperature of the continuous casting tundish (with flame) is 1220℃. Before pouring, add calcium wire to the tundish (do not cut it, just put it in small bundles), add 10m of calcium wire to each baking hole near the flow, and add 20m of calcium wire to the steel mouth.
[0035] (6) In order to reduce the secondary oxidation of molten steel, argon blowing control should be implemented in all links:
[0036] a. Before pouring, the tundish is moving, and argon is blown into the tundish body using an elbow argon blowing pipe at 1800L / min for 4 minutes;
[0037] b. The tundish arrives at the casting position, and the tundish is blown with argon at the steel mouth at 250L / min for 3 minutes;
[0038] c. Argon blowing of 150L / min at the ladle slide mechanism during the pouring process;
[0039] d. Argon blowing at 350L / min through the argon sealing ring of the ladle's long nozzle during the pouring process;
[0040] (7) The molten steel in the tundish is covered with a heat-insulating method that combines magnesium covering agent with carbonized rice husk. The covering agent is sufficient and dedicated personnel are assigned to add the covering agent on both sides of the tundish. When the weight of the molten steel in the first furnace reaches about 7 tons, about 50 kg of magnesium covering agent is added to each baking hole in the non-impact area (the reference addition amount of 5 kg bags is 10 bags). When the weight of the molten steel in the tundish reaches 18 tons, about 100 kg of magnesium covering agent is added to the steel receiving port (the reference addition amount of 5 kg bags is 20 bags). The amount of magnesium covering added to the tundish of the first furnace is not less than 400 kg (i.e. 80 bags).
[0041] (8) Before pouring the ladle, the stopper rod of the intermediate ladle should be tested in advance to ensure reliable operation of the mechanism.
[0042] (9) All casting modes adopt the manual small steel flow steady pressure starting method, and the starting casting speed is uniformly set at 1.0m / min.
[0043] Low-carbon cold heading steel can be directly cast in the billet continuous casting machine with a success rate of 100%.
[0044] Example 2
[0045] A direct casting process for billet low-carbon cold-heading steel is described. The production process includes: converter process - argon station process - LF process - billet continuous casting process. The Al content in the molten steel is controlled in the argon station process, the temperature, Al content, Si content and Ca content of the molten steel are controlled in the LF process, the baking temperature of the continuous casting tundish is controlled, argon blowing is controlled in each step of the continuous casting process, a covering agent is added to the tundish, and the casting speed is stably controlled, ultimately achieving direct casting of billet low-carbon cold-heading steel. Specifically:
[0046] (1) The clearance of the ladle is 350mm (including the vertical brick of the ladle mouth) to reduce the spraying of molten steel when feeding the Ca wire.
[0047] (2) Control the Al content in the molten steel at the argon station to 0.050%.
[0048] (3) According to sample 1, add Al to 0.045%, and try not to add aluminum later. According to sample 2, add Si to 0.065%; before feeding the Ca line, control the Al content to about 0.046%, the temperature reference: 1620℃, control the outgoing Al content to about 0.035%, Si content to 0.07%, and Ca content to 38ppm (target 35-45ppm).
[0049] (4) The outlet temperature of molten steel in the LF process is TL+75℃, and the reference temperature of the continuous casting platform is TL+70℃ to ensure that the superheat of the tundish is between 37-45℃.
[0050] (5) The baking temperature of the continuous casting tundish (with flame) is 1250℃. Before pouring, add calcium wire to the tundish (do not cut it, just put it in small bundles), add 10m of calcium wire to each baking hole near the flow, and add 20m of calcium wire to the steel mouth.
[0051] (6) In order to reduce the secondary oxidation of molten steel, argon blowing control should be implemented in all links:
[0052] a. Before pouring, the tundish is moving, and argon is blown into the tundish body using an elbow argon blowing pipe at 1800L / min for 5 minutes;
[0053] b. The tundish arrives at the casting position, and the tundish is blown with argon at the steel mouth at 250L / min for 3 minutes;
[0054] c. Argon blowing of 150L / min at the ladle slide mechanism during the pouring process;
[0055] d. Argon blowing at 350L / min through the argon sealing ring of the ladle's long nozzle during the pouring process;
[0056] (7) The molten steel in the tundish is covered with a heat-insulating method that combines magnesium covering agent with carbonized rice husk. The covering agent is sufficient and dedicated personnel are assigned to add the covering agent on both sides of the tundish. When the weight of the molten steel in the first furnace reaches about 7 tons, about 50 kg of magnesium covering agent is added to each baking hole in the non-impact area (the reference addition amount of 5 kg bags is 10 bags). When the weight of the molten steel in the tundish reaches 18 tons, about 100 kg of magnesium covering agent is added to the steel receiving port (the reference addition amount of 5 kg bags is 20 bags). The amount of magnesium covering added to the tundish of the first furnace is not less than 400 kg (i.e. 80 bags).
[0057] (8) Before pouring the ladle, the stopper rod of the intermediate ladle should be tested in advance to ensure reliable operation of the mechanism.
[0058] (9) All casting modes adopt the manual small steel flow steady pressure starting method, and the starting casting speed is uniformly set at 1.0m / min.
[0059] Low-carbon cold heading steel can be directly cast in the billet continuous casting machine with a success rate of 100%.
[0060] Comparative Example 1
[0061] The steps were similar to those in Example 1, except that the Al content in the molten steel at the argon station was 0.020%. This low Al content prevented sufficient oxygen removal from the molten steel, resulting in a high concentration of oxides in subsequent molten steel treatments. Frequent liquid level fluctuations during the pouring process led to failed pouring runs, resulting in a pouring success rate of 92.85%.
[0062] Comparative Example 2
[0063] The steps were similar to those in Example 1, except that the Al content in the molten steel during the LF process was 0.035%, and Al was subsequently added. The deoxidation product, Al2O3, formed during the subsequent Al addition did not have sufficient time to float up, resulting in its retention in the molten steel. During the pouring process, Al2O3 accumulated at the stopper nozzle, causing frequent liquid level fluctuations and leading to failed pouring. The pouring success rate was 95.23%.
[0064] Comparative Example 3
[0065] The steps were similar to those in Example 1, except that the Ca content in the molten steel leaving the LF station was 20 ppm. Insufficient Ca treatment resulted in insufficient conversion of inclusions into low-melting-point 12CaO7·Al2O3 in the molten steel. High-melting-point inclusions accumulated at the stopper nozzle, leading to nozzle nodules and failure of some runs. The success rate was 85.14%.
[0066] Comparative Example 4
[0067] The steps were similar to those in Example 1, except that no argon purge was performed during the continuous casting start. The tundish was filled with oxidizing air. The oxygen in the air reacted with elements such as Al in the molten steel during the ladle pouring process, causing severe oxidation of the molten steel during the pouring process. This generated a large amount of Al₂O₃ inclusions. The high-melting-point Al₂O₃ accumulated at the stopper nozzle, blocking it and causing some casting runs to fail. The pouring success rate was 89.53%.
[0068] Comparative Example 5
[0069] The steps were similar to those in Example 1, differing only in that the initial casting speed for continuous casting was not uniformly set; some runs had a lower initial casting speed of 0.60 m / min, while others had a higher initial casting speed of 1.10 m / min. A too low initial casting speed could easily lead to dead flow during the casting process, while a too high initial casting speed could result in a thin, insufficiently strong shell and prone to leaking, leading to casting failure. The casting success rate was 96.5%.
[0070] From the foregoing, it can be seen that an embodiment of the present invention provides a production process for direct casting of low-carbon cold-heading steel in small square billets, including: optimizing the Al control method for the steel grade in the LF process to ensure that molten steel deoxidation is completed as soon as possible, allowing sufficient time for the deoxidation product Al2O3 to float. Optimizing the Si content in the molten steel to minimize the [O] content in the molten steel and reduce Al2O3 formation. Optimizing the Ca processing capacity of the molten steel to control the outgoing Ca content to 30-45ppm. The higher Ca content in the molten steel can react with Al2O3 in the molten steel to form a low-melting-point 12CaO7·Al2O3, thereby preventing nozzle nodules. Simultaneously, ensuring continuous casting and pouring operations are properly protected, effectively improving the success rate of direct casting of low-carbon cold-heading steel in small square billets.
[0071] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Those skilled in the art will readily appreciate that various modifications and variations of the present invention are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention shall be included within the scope of protection of the present invention.
Claims
1. A production process for direct casting of low-carbon cold heading steel billets, characterized in that: The production process of small square billet low carbon cold heading steel includes: converter process-argon station process-LF process-small square billet continuous casting process, and the Al content in the molten steel is controlled in the argon station process, the temperature, Al content, Si content and Ca content of the molten steel are controlled in the LF process, the baking temperature of the continuous casting tundish is controlled, argon blowing control is implemented in each link of continuous casting, covering agent is added in the tundish, and the casting speed is stably controlled, finally realizing the direct casting of small square billet low carbon cold heading steel.
2. The production process of direct casting of low-carbon cold heading steel for small square billets according to claim 1 is characterized in that: Controlling the Al content in the molten steel in the argon station process includes: controlling the Al content in the molten steel in the argon station to be 0.030-0.060%.
3. The production process of direct casting of low-carbon cold heading steel for small square billets according to claim 1 is characterized in that: Controlling the Al content, Si content and Ca content in molten steel in the LF process includes: first controlling the ladle clearance ≥ 300mm, and the ladle clearance includes the vertical bricks at the ladle mouth to reduce the molten steel spraying when feeding the calcium line, and adding Al to 0.045-0.050% according to sample 1, and try not to add aluminum later, and adding Si to 0.065% according to sample 2.
4. The production process for direct casting of low-carbon cold heading steel billet according to claim 3 is characterized in that: Also includes: After aluminum supplementation and before feeding the calcium wire, the molten steel temperature is controlled at 1620°C and the Al content is 0.046%. Then the calcium wire is fed and soft blowing is performed, so that the Ca content in the LF outgoing molten steel is 30-45ppm, the Al content is 0.031%, and the Si content is 0.07-0.09%.
5. The production process for direct casting of low-carbon cold heading steel billet according to claim 1, characterized in that: Controlling the temperature of molten steel in the LF process includes: controlling the molten steel temperature at the LF exit to TL+75°C and the molten steel temperature on the continuous casting platform to TL+70°C, to ensure that the superheat of the tundish is 37-45°C, where TL is the liquidus temperature of the molten steel.
6. The production process of direct casting of low-carbon cold heading steel for small square billets according to claim 1 is characterized in that: Controlling the baking temperature of the continuous casting tundish includes: controlling the baking temperature of the continuous casting tundish to 1200-1250℃, adding calcium wire to the tundish before pouring, the addition amount near the flow baking hole is 10m, and the addition amount at the steel receiving mouth is 20m.
7. The production process of direct casting of low-carbon cold heading steel for small square billets according to claim 1 is characterized in that: The implementation of argon blowing control in each link to reduce secondary oxidation of molten steel includes: a. During the movement of the tundish car before pouring, argon is blown into the tundish body with an elbow argon blowing pipe at 1800L / min for a duration of more than 3 minutes; b. The tundish car arrives at the casting position, and the tundish is blown with argon at the steel mouth at 250L / min for a duration of >2min; c. The ladle slide mechanism is blown with argon at 150L / min during the pouring process; d. The argon sealing ring of the long water nozzle of the large ladle is blown with argon at 350L / min during the pouring process.
8. The production process for direct casting of low-carbon cold heading steel billet according to claim 1, characterized in that: The covering agent added in the tundish includes: the molten steel in the tundish is covered with a heat-insulating method combining a magnesium covering agent and carbonized rice husk. When the weight of the molten steel in the tundish of the first furnace reaches about 7t, 50Kg of magnesium covering agent is added to each baking hole in the non-impact zone. When the weight of the molten steel in the tundish reaches 18t, 100Kg of magnesium covering agent is added to the steel receiving port. When pouring the first furnace tundish, no less than 400Kg of magnesium covering agent is added.
9. The production process for direct casting of low-carbon cold heading steel billet according to claim 1, characterized in that: Also includes: Before pouring the ladle, the stopper rod of the tundish is tested in advance to ensure reliable operation of the mechanism.
10. The production process of direct casting of low-carbon cold heading steel for small square billets according to claim 1, characterized in that: Stable control of casting speed includes: all casting modes adopt manual small steel flow steady pressure starting method, and the starting casting speed is uniformly set to 1.0m / min.