Preparation method of efficient condenser pipe for heat exchanger
By grinding copper powder and yttrium powder in a ball mill, adding zirconium oxide fibers, vacuum hot press sintering and upsetting forging, the problem of poor corrosion resistance of copper alloy condensate tubes in harsh environments is solved, and the thermal conductivity and mechanics are improved Performance extends the service life of the condensate tube.
Patent Information
- Application Number
- CN202410920777.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
AI Technical Summary
The existing copper alloy condenser tubes have poor corrosion resistance, reduced thermal conductivity and high cost in harsh environments, so their performance needs to be improved to extend their service life.
By mechanically grinding pure copper powder, high-purity yttrium powder and other metal powders in a ball mill, a spherical powder is formed, zirconia fibers are added, vacuum hot press sintering and multiple upsetting forging, refine the grains, and improve thermal conductivity and resistance. Corrosive.
It significantly improves the thermal conductivity, mechanical properties and corrosion resistance of the condenser tube, and extends the service time of the condenser tube.
Smart Images

Figure BDA0004936642810000041 
Figure BDA0004936642810000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of condenser tubes, and in particular to a method for preparing a high-efficiency condenser tube for a heat exchanger. Background Art
[0002] Heat exchangers are a kind of general equipment widely used in chemical industry, oil refining, power, food, light industry, atomic energy, pharmaceutical, machinery and many other industrial sectors, and they play an important role in production. In chemical production, heat exchangers can be used as heaters, coolers, condensers, evaporators and reboilers, etc., and are more widely used.
[0003] In the past, copper with excellent thermal conductivity was used for condensers in heat exchangers such as water heaters, air conditioners (air conditioners, air conditioning equipment, etc.), freezers, cold storages, etc. Copper alloys have many valuable physical and chemical properties, such as high thermal conductivity and electrical conductivity, strong chemical stability, high tensile strength, easy welding, good corrosion resistance, and excellent plasticity and ductility. As an important basic material and functional material, it has been widely used in the development of the national economy. In my country, it is the second largest non-ferrous metal consumed after aluminum alloy. However, the corrosion resistance of copper alloys, especially in alkaline conditions or high-temperature and high-oxygen environments, is poor, and the hardness is average and the wear resistance is poor, so it will fail quickly in harsh environments. In addition, the price of copper alloys is relatively high, so it is even more necessary to further improve their performance and protect them. At present, although most copper alloys have sufficient strength, their thermal conductivity is greatly reduced. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a high-efficiency condenser tube for a heat exchanger, so as to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing a high-efficiency condenser tube for a heat exchanger, comprising the following preparation steps:
[0006] (1) Pure copper powder and high-purity yttrium powder are added to a planetary high-energy ball mill at a ball mill speed of 600 to 1000 rpm. The grinding balls are stainless steel balls. The ball mill is milled for 6 to 10 hours. After each ball milling for 1.5 to 2.5 hours, metal tungsten powder, metal nickel powder, zinc powder, and silicon powder are added in sequence. The ball mill speed is adjusted to 300 to 400 rpm. 1 / 2 weight of zirconia fiber is added. After ball milling for 10 to 15 minutes, the remaining 1 / 2 weight of zirconia fiber is added. The ball mill is milled for 20 minutes to obtain a condenser precursor powder.
[0007] (2) Pour the condenser precursor powder into a mold, cold press it into shape, put it into a vacuum hot press sintering machine, heat and press it under certain vacuum conditions, and sinter it for 5-30 minutes to obtain a blank;
[0008] (3) The blank is kept at 880-1000°C for 4.5h-5h, subjected to multiple upsetting and drawing forging, each of which is subjected to diagonal drawing, annealed at 850°C for 2h, drilled, and then subjected to multiple hot rolling at 750-800°C, followed by homogenization annealing to obtain a high-efficiency condenser tube for a heat exchanger.
[0009] Furthermore, in step (1), the weight ratio of the copper powder, high-purity yttrium powder, tungsten powder, nickel powder, zinc powder, silicon powder and zirconium oxide fiber is 90-98: 0.02-0.4: 0.2-1: 0.01-0.15: 0.001-0.5: 0.001-0.5: 0.1-3.
[0010] Furthermore, the metal tungsten, copper powder, high-purity yttrium powder, metal nickel powder, zinc powder, and silicon powder in step (1) all have a particle size of 200 μm.
[0011] Furthermore, the zirconia fiber in step (1) has a length of 3 to 5 mm and a diameter of 50 to 150 μm.
[0012] Furthermore, in the entire ball milling process of step (1), the ball-to-material weight ratio is maintained at 3 to 6:1.
[0013] Furthermore, the vacuum condition in step (2) is: 100-1Pa~10-2Pa.
[0014] Furthermore, the temperature in step (2) is 1200-1400° C. and the pressure is 20-40 MPa.
[0015] Furthermore, the homogenization annealing in step (3) is specifically as follows: the first stage heating temperature is 380-460° C., and the heat preservation is 1-5 hours; the second stage heating temperature is 500-545° C., and the heat preservation is 1-5 hours; the third stage heating temperature is 550-580° C., and the heat preservation is 4-10 hours.
[0016] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0017] The present invention successively adds high-purity yttrium powder, tungsten powder, nickel powder, zinc powder, silicon powder and copper powder for mechanical grinding, and irregular edges and corners are removed to make them spherical, which can reduce the agglomeration between metal powders. At the same time, each element and Cu are initially mechanically alloyed, and the processing activity is improved, which is beneficial to improve the mechanical properties of the condenser. In addition, the particle size of each metal powder is adjusted by the order of adding successively, and the metal powders with different particle sizes are matched with each other, and the metal powders are uniformly contacted with copper and effectively filled, and the growth of grains can be effectively inhibited during the sintering process. After the grinding is completed, zirconium oxide fibers are added in batches for secondary grinding. The addition of zirconium oxide fibers can form a skeleton structure inside the alloy. The structure has a reinforcing effect. At the same time, with the grinding process, the contact area with copper is smaller, the heat conduction is less hindered, and the thermal conductivity is better. In addition, the metal powder and zirconia fiber are combined in different lengths and different particle sizes, which can effectively improve the density of the alloy condenser, improve the thermal conductivity and heat dissipation of the condenser and the comprehensive mechanical properties. Zr and Ni, Zn, Y, Si, W cooperate with each other, which can significantly refine the grains of the copper alloy and make the grains uniform, which can effectively improve the corrosion resistance and processing performance of the condenser. Combined with the processing technology, the grains are refined, so that the mechanical strength, thermal conductivity and corrosion resistance of the copper alloy are optimized, and the service life of the condenser is extended. DETAILED DESCRIPTION
[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0019] Example 1
[0020] (1) adding pure copper powder and high-purity yttrium powder to a planetary high-energy ball mill, the ball mill speed is 600 rpm, the grinding balls are stainless steel balls, and the ball milling is performed for 6 hours. After each ball milling for 1.5 hours, metal tungsten powder, metal nickel powder, zinc powder, and silicon powder are added in sequence, and the ball mill speed is adjusted to 300 rpm. 1 / 2 weight of zirconia fiber is added. After ball milling for 10 minutes, the remaining 1 / 2 weight of zirconia fiber is added and ball milled for 20 minutes. The weight ratio of the ball to the material is maintained at 4:1 throughout the process to obtain a condenser precursor powder; the weight ratio of the copper powder, high-purity yttrium powder, tungsten powder, nickel powder, zinc powder, silicon powder, and zirconia fiber is 90:0.1:0.2:0.06:0.023:0.1:0.1; the zirconia fiber has a length of 3 mm and a diameter of 150 μm;
[0021] (2) Pour the condenser precursor powder into a mold, cold press it into shape, put it into a vacuum hot press sintering machine, heat and press it under a vacuum condition of 100-1Pa, the sintering temperature is 1280°C, the pressure is 25MPa, and the sintering time is 30min to obtain a blank;
[0022] (3) The tube blank is subjected to four times of upsetting and drawing forging, the first time is upsetting and drawing forging at 1000°C and holding temperature for 5h, the second time is upsetting and drawing forging at 960°C and holding temperature for 4.5h, the third time is upsetting and drawing forging at 920°C and holding temperature for 5h, and the fourth time is upsetting and drawing forging at 880°C and holding temperature for 5h. Each time is subjected to diagonal drawing to obtain a bar with a specification of Φ50mm, which is annealed at 850°C for 2h, drilled, and obtained to obtain a tube with a specification of Φ50×6mm, and then hot rolled at 800°C for multiple passes to obtain a tube with a specification of Φ12.7×0.6mm, and then homogenized annealing is performed: the first stage heating temperature is 380°C, holding temperature is 3h, the second stage heating temperature is 500°C, holding temperature is 3h, and the third stage heating temperature is 550°C, holding temperature is 5.5h, and the high-efficiency condenser tube for heat exchanger is obtained.
[0023] Example 2
[0024] (1) adding pure copper powder and high-purity yttrium powder to a planetary high-energy ball mill, the ball mill speed is 800 rpm, the grinding balls are stainless steel balls, and the ball milling is performed for 8 hours. After each ball milling for 2 hours, metal tungsten powder, metal nickel powder, zinc powder, and silicon powder are added in sequence, and the ball mill speed is adjusted to 300 rpm. 1 / 2 weight of zirconia fiber is added, and after ball milling for 12 minutes, the remaining 1 / 2 weight of zirconia fiber is added, and the ball milling is performed for 20 minutes. The weight ratio of the ball to the material is maintained at 4:1 throughout the process to obtain a condenser precursor powder; the weight ratio of the copper powder, high-purity yttrium powder, tungsten powder, nickel powder, zinc powder, silicon powder, and zirconia fiber is 94:0.21:0.2:0.08:0.2:0.14:1.2; the zirconia fiber has a length of 3 mm and a diameter of 150 μm;
[0025] (2) Pour the condenser precursor powder into a mold, cold press it into shape, put it into a vacuum hot press sintering machine, heat and press it under a vacuum condition of 100-1Pa, the sintering temperature is 1280°C, the pressure is 25MPa, and the sintering time is 30min to obtain a blank;
[0026] (3) The tube blank is subjected to four times of upsetting and drawing forging, the first time is upsetting and drawing forging at 1000°C and holding temperature for 5h, the second time is upsetting and drawing forging at 960°C and holding temperature for 4.5h, the third time is upsetting and drawing forging at 920°C and holding temperature for 5h, and the fourth time is upsetting and drawing forging at 880°C and holding temperature for 5h. Each time is subjected to diagonal drawing to obtain a bar with a specification of Φ50mm, which is annealed at 850°C for 2h, drilled, and obtained into a tube with a specification of Φ50×6mm. It is then subjected to multiple hot rolling at 800°C to obtain a tube with a specification of Φ12.7×0.6mm, and then subjected to homogenization annealing: the first stage heating temperature is 420°C, holding temperature is 3h, the second stage heating temperature is 520°C, holding temperature is 3h, and the third stage heating temperature is 570°C, holding temperature is 7h, and a high-efficiency condenser tube for heat exchanger is obtained.
[0027] Example 3
[0028] (1) adding pure copper powder and high-purity yttrium powder to a planetary high-energy ball mill, the ball mill speed is 800 rpm, the grinding balls are stainless steel balls, and the ball milling is performed for 8 hours. After each ball milling for 2.5 hours, metal tungsten powder, metal nickel powder, zinc powder, and silicon powder are added in sequence, and the ball mill speed is adjusted to 400 rpm. 1 / 2 weight of zirconia fiber is added, and after ball milling for 15 minutes, the remaining 1 / 2 weight of zirconia fiber is added, and the ball milling is performed for 20 minutes. The weight ratio of the ball to the material is maintained at 4:1 throughout the process to obtain a condenser precursor powder; the weight ratio of the copper powder, high-purity yttrium powder, tungsten powder, nickel powder, zinc powder, silicon powder, and zirconia fiber is 98:0.4:1:0.09:0.2:0.32:2.1; the zirconia fiber has a length of 3 mm and a diameter of 150 μm;
[0029] (2) Pour the condenser precursor powder into a mold, cold press it into shape, put it into a vacuum hot press sintering machine, heat and press it under a vacuum condition of 100-1Pa, the sintering temperature is 1280°C, the pressure is 25MPa, and the sintering time is 30min to obtain a blank;
[0030] (3) The tube blank is subjected to 4 times of upsetting and drawing forging, the first time is upsetting and drawing forging at 1000°C and holding temperature for 5h, the second time is upsetting and drawing forging at 960°C and holding temperature for 4.5h, the third time is upsetting and drawing forging at 920°C and holding temperature for 5h, and the fourth time is upsetting and drawing forging at 880°C and holding temperature for 5h. Each time is subjected to diagonal drawing to obtain a bar with a specification of Φ50mm, which is annealed at 850°C for 2h, drilled, and obtained into a tube with a specification of Φ50×6mm. It is then subjected to multiple hot rolling at 800°C to obtain a tube with a specification of Φ12.7×0.6mm, and then subjected to homogenization annealing: the first stage heating temperature is 460°C, holding temperature is 2.5h, the second stage heating temperature is 545°C, holding temperature is 2.5h, and the third stage heating temperature is 580°C, holding temperature is 4h, and high-efficiency condenser tubes for heat exchangers are obtained.
[0031] Comparative Example 1
[0032] The difference between Comparative Example 1 and Example 2 is that zirconium oxide fiber is not added, and the remaining steps are the same as Example 2.
[0033] Comparative Example 2
[0034] The difference between Comparative Example 2 and Example 2 is that high-purity yttrium powder is not added, and the remaining steps are the same as Example 2.
[0035] Comparative Example 3
[0036] The difference between Comparative Example 3 and Example 2 is that metal tungsten powder is not added, and the remaining steps are the same as Example 2.
[0037] Comparative Example 4
[0038] The difference between Comparative Example 4 and Example 2 is that no metal nickel powder is added, and the remaining steps are the same as Example 2.
[0039] Comparative Example 5
[0040] The difference between Comparative Example 5 and Example 2 is that silicon powder is not added, and the remaining steps are the same as Example 2.
[0041] Comparative Example 6
[0042] The difference between Comparative Example 6 and Example 2 is that zinc powder is not added, and the remaining steps are the same as Example 2.
[0043] Comparative Example 7
[0044] The difference between Comparative Example 7 and Example 2 is that step (1) is different. Step (1) is changed to: pure copper powder, high-purity yttrium powder, tungsten powder, nickel powder, zinc powder, silicon powder, and zirconium oxide fiber are added into a planetary high-energy ball mill in a weight ratio of 94:0.21:0.2:0.08:0.2:0.14:1.2. The ball mill speed is 800 rpm, the grinding balls are stainless steel balls, and the ball milling is carried out for 8 hours. The remaining steps are the same as Example 2.
[0045] Effect example
[0046] Table 1 below shows the performance analysis results of the condenser tubes of Examples 1 to 3 of the present invention and Comparative Examples 1 to 7.
[0047] Table 1
[0048]
[0049]
[0050] From the comparison of the experimental data of the embodiments and the comparative examples, it can be found that the metal powder and the zirconium oxide fiber in the present invention are in a combination of different lengths and different particle sizes, which can effectively improve the density of the alloy condenser, improve the thermal conductivity, heat dissipation and comprehensive mechanical properties of the condenser, and the metal elements cooperate with each other to significantly refine the grains of the copper alloy and make the grains uniform, which can effectively improve the corrosion resistance and processing performance of the condenser, and then with the processing technology, the grains are refined, so that the mechanical strength, thermal conductivity and corrosion resistance of the copper alloy are optimized, thereby extending the service life of the condenser.
[0051] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing a high-efficiency condenser tube for a heat exchanger, characterized in that: The method comprises the following preparation steps: (1) Pure copper powder and high-purity yttrium powder are added to a planetary high-energy ball mill at a ball mill speed of 600 to 1000 rpm. The grinding balls are stainless steel balls. The ball mill is milled for 6 to 10 hours. After each ball milling for 1.5 to 2.5 hours, metal tungsten powder, metal nickel powder, zinc powder, and silicon powder are added in sequence. The ball mill speed is adjusted to 300 to 400 rpm. 1 / 2 weight of zirconia fiber is added. After ball milling for 10 to 15 minutes, the remaining 1 / 2 weight of zirconia fiber is added. The ball mill is milled for 20 minutes to obtain a condenser precursor powder. (2) Pour the condenser precursor powder into a mold, cold press it into shape, put it into a vacuum hot press sintering machine, heat and press it under certain vacuum conditions, and sinter it for 5-30 minutes to obtain a blank; (3) The blank is kept at 880-1000°C for 4.5h-5h, subjected to multiple upsetting and drawing forging, each of which is subjected to diagonal drawing, annealed at 850°C for 2h, drilled, and then subjected to multiple hot rolling at 750-800°C, followed by homogenization annealing to obtain a high-efficiency condenser tube for a heat exchanger.
2. The method for preparing a high-efficiency condenser tube for a heat exchanger according to claim 1, characterized in that: The weight ratio of the copper powder, high-purity yttrium powder, tungsten powder, nickel powder, zinc powder, silicon powder and zirconium oxide fiber in step (1) is 90-98: 0.02-0.4: 0.2-1: 0.01-0.15: 0.001-0.5: 0.001-0.5: 0.1-3.
3. The method for preparing a high-efficiency condenser tube for a heat exchanger according to claim 1, characterized in that: The metal tungsten, copper powder, high-purity yttrium powder, metal nickel powder, zinc powder and silicon powder in step (1) all have a particle size of 200 μm.
4. The method for preparing a high-efficiency condenser tube for a heat exchanger according to claim 1, characterized in that: The zirconia fiber in step (1) has a length of 3 to 5 mm and a diameter of 50 to 150 μm.
5. The method for preparing a high-efficiency condenser tube for a heat exchanger according to claim 1, characterized in that: In step (1), the ball-to-material weight ratio is maintained at 3 to 6:1 throughout the ball milling process.
6. The method for preparing a high-efficiency condenser tube for a heat exchanger according to claim 1, characterized in that: The vacuum condition in step (2) is: 100-1Pa~10-2Pa.
7. The method for preparing a high-efficiency condenser tube for a heat exchanger according to claim 1, characterized in that: The temperature in step (2) is 1200-1400° C. and the pressure is 20-40 MPa.
8. The method for preparing a high-efficiency condenser tube for a heat exchanger according to claim 1, characterized in that: The homogenization annealing in step (3) is specifically as follows: the first stage heating temperature is 380-460°C, and the heat preservation is 1-5 hours; the second stage heating temperature is 500-545°C, and the heat preservation is 1-5 hours; the third stage heating temperature is 550-580°C, and the heat preservation is 4-10 hours.