Integral machining method for complex aluminum alloy pagoda-shaped part

By adopting multi-stage aging treatment and five-axis machining center combined with tooling fixture bonding technology in the processing of pagoda aluminum alloy parts, the vibration and vibration problems caused by poor structural rigidity during the processing process are solved, and high precision and efficiency are achieved. Processing effect.

CN118875651APending Publication Date: 2024-11-01三河建华高科有限责任公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410958225.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

During the processing process, pagoda-shaped aluminum alloy parts have poor rigidity due to their high center and thin wall structure, which is prone to trembling and vibration, resulting in increased processing difficulty. Especially under the processing requirements of high precision and complex contours, it is difficult to effectively control the thermal effect and improve. Dynamic stability.

Method used

Using 7075-T651 aluminum alloy rods, through rough turning, rough milling, semi-finishing, semi-finishing milling, liquid nitrogen low-temperature aging treatment and grinding reference surfaces, combined with five-axis machining center and tooling fixtures, use bonding technology and foam filling The object can stabilize the positioning of parts, gradually reduce the processing allowance and release stress, and improve processing stability.

Benefits of technology

It significantly improves the processing stability and accuracy of aluminum alloy pagoda-shaped parts, reduces labor strength and material removal rate, and ensures processing quality and long-term stability of finished products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118875651A_ABST
    Figure CN118875651A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of aluminum alloy machining, and provides a complex aluminum alloy pagoda-shaped part overall machining method which comprises the following steps that S1, imported aluminum alloy bars are adopted; s2, rough turning; s3, performing high-temperature aging treatment; s4, performing semi-finish turning on each outer circle for the first time, and performing rough milling on four sides and each square hole; s5, medium-temperature aging treatment is carried out; s6, each outer circle is subjected to semi-finish turning again, and four sides and each square hole are subjected to semi-finish milling; s7, liquid nitrogen low-temperature aging treatment is conducted; s8, performing finish turning on each outer circle, and performing finish milling on four sides and each square hole; s9, grinding the reference surface; by means of the steps, the problem that deformation and vibration are large during overall machining and clamping of the complex tower-shaped parts is ingeniously solved, and when pagoda-shaped parts which are small and medium in batch, difficult to clamp and align, large in material removal amount and large in deformation and vibration are machined, the machining and clamping method and the heat treatment process are unique, tools are simple, the labor intensity is lowered, and the machining quality and efficiency are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of aluminum alloy processing, in particular to an integral processing method for complex aluminum alloy pagoda-shaped parts. Background Art

[0002] As an engineering material, aluminum alloy has been widely used in aviation, electronics, automobile manufacturing and other fields due to its low density, high strength and good corrosion resistance. Especially with the trend of pursuing lightweight design, the demand for aluminum alloy parts is growing. Pagoda-shaped aluminum alloy parts are often used in designs that require high-strength support and weight reduction due to their unique geometric structure, such as casings of precision electronic equipment, aerospace structural parts, etc.

[0003] The processing of existing pagoda-shaped parts faces many challenges. These parts are usually processed from a whole piece of aluminum rod by removing a large amount of material. The high material removal rate (up to 80%) means that a large amount of cutting heat will be generated during the processing, which will not only easily lead to local overheating of the workpiece, but also cause thermal deformation, affecting dimensional accuracy and shape consistency; in addition, the structural characteristics of pagoda-shaped parts, such as high center and thin wall, result in poor rigidity during processing, and are prone to chatter and vibration, further exacerbating the difficulty of processing.

[0004] Traditional processing strategies, such as strong clamping, optimizing tool paths, and using coolants, can alleviate these problems to a certain extent, but it is often difficult to fundamentally solve the problem of large processing vibration and deformation, especially under the requirements of high-precision and complex contour processing. How to effectively control the thermal effects during processing and improve the dynamic stability of the workpiece during processing has become the key to improving the processing quality of aluminum alloy pagoda-shaped parts.

[0005] To this end, those skilled in the art have proposed an overall processing method for complex aluminum alloy pagoda-shaped parts to solve the problems raised by the background technology. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides an overall processing method for complex aluminum alloy pagoda-shaped parts to solve the structural characteristics of pagoda-shaped parts in the prior art, such as high center, thin wall, etc., which result in poor rigidity during processing, easy to vibrate and shake, further aggravating the processing difficulty and other problems.

[0007] A method for integrally processing a complex aluminum alloy pagoda-shaped part comprises the following steps:

[0008] S1. Use 7075-T651 imported aluminum alloy bars;

[0009] S2, Rough Turning and Each outer circle;

[0010] S3, high temperature aging treatment;

[0011] S4, first semi-finish turning of all outer circles, rough milling of four squares and square holes;

[0012] S5, performing medium temperature aging treatment;

[0013] S6, semi-finish turning each outer circle again, semi-finish milling the four squares and each square hole;

[0014] S7, performing liquid nitrogen low temperature aging treatment;

[0015] S8, precision turning of all outer circles, precision milling of four squares and square holes;

[0016] S9, grinding the reference surface to a flatness of 0.005 and obtaining the processing technology benchmark;

[0017] S10. Using the grinding reference surface as the reference, the five-axis machining center processes the square and square holes, and the holes in relative positions to obtain the accuracy required by the drawing for each hole.

[0018] Preferably, a fixture, a secondary pressure plate support column and a main pressure plate support column are installed on the upper surface of the workbench of the five-axis machining center, a main pressure plate is installed on the top wall of the main pressure plate support column, and a secondary pressure plate is installed on the top wall of the secondary pressure plate support column. The surfaces of the main pressure plate and the secondary pressure plate are both installed with clamping screws, and the bottom end of the clamping screw is connected to the positioning groove of the workbench of the five-axis machining center;

[0019] A viscose substrate support block is also installed on the upper surface of the workbench of the five-axis machining center. The upper surface of the viscose substrate support block supports a viscose substrate, and the viscose substrate is located below the secondary pressing plate.

[0020] Preferably, the rough turning in S2 leaves a single-sided semi-finishing allowance of 2-3 mm, the purpose of which is to remove most of the machining allowance and prepare for the subsequent semi-finishing turning and milling.

[0021] Preferably, the first semi-finishing turning in S4 leaves a single-sided semi-finishing allowance of 1-2 mm to prepare for subsequent finishing turning and milling.

[0022] Preferably, the medium-temperature aging treatment in S5 is performed by heating to 220° C.-180° C. and keeping the temperature for 12 hours to further release stress.

[0023] Preferably, in the second semi-finishing turning in S6, a semi-finishing allowance of 1 mm is left on one side to prepare for final finishing.

[0024] Preferably, the low-temperature aging treatment in S7 is performed by placing the steel sheet in liquid nitrogen at -40°C for 36 hours to further stabilize the size.

[0025] Preferably, in the finish turning in S8, a single-sided semi-finishing allowance of 0.5 mm is left to prepare for final finishing.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The present invention performs rough turning, rough milling, semi-finishing turning, semi-finishing milling, grinding the reference surface and the tooling positioning surface, and finally finishing turning, with three medium and low temperature aging treatments interspersed in between, specifically, stress relief aging treatment is performed after rough turning, medium temperature aging treatment is performed after semi-finishing, and liquid nitrogen low temperature aging treatment is performed after semi-finishing and before finishing. In finishing, the reference surface is ground first, and then the milling clamping stability of the part is greatly increased through clamping tooling cooperation and bonding, which ingeniously solves the problem of large deformation and vibration of the overall processing clamping of complex tower-shaped parts. When the pagoda-shaped parts are small and medium batches, difficult to clamp and align, require a lot of material to be removed, and have large deformation and vibration, the processing clamping method and heat treatment process are unique, the tooling is simple, the labor intensity is reduced, and the processing quality and efficiency are improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a process flow chart of the present invention;

[0029] Figure 2 It is a schematic diagram of the overall structure of the clamping tool of the present invention.

[0030] In the figure:

[0031] 1. Five-axis machining center workbench; 2. Glue substrate support block; 3. Secondary pressure plate support column; 4. Secondary pressure plate; 5. Glue substrate; 6. Parts to be processed; 7. Auxiliary glue; 8. Fixture; 9. Clamping screw; 10. Main pressure plate; 11. Main pressure plate support column. DETAILED DESCRIPTION

[0032] The following is a further detailed description of the embodiments of the present invention in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.

[0033] Embodiment 1: As shown in the attached Figure 1 To Attachment Figure 2 As shown: The present invention provides a method for integrally processing a complex aluminum alloy pagoda-shaped part, comprising the following steps:

[0034] S1. Use 7075-T651 imported aluminum alloy bars;

[0035] S2, Rough Turning and For each outer circle, leave a single-sided semi-finishing allowance of 2-3mm, the purpose is to remove most of the machining allowance and prepare for the subsequent semi-finishing turning and milling;

[0036] S3, high temperature aging treatment;

[0037] S4. Semi-finish turning of each outer circle for the first time, rough milling of four squares and square holes, leaving a single-sided semi-finishing allowance of 1-2mm to prepare for subsequent finishing and milling.

[0038] S5. Perform medium temperature aging treatment, heating to 220℃-180℃ and keeping warm for 12 hours to further release stress;

[0039] S6, semi-finish turning each outer circle again, semi-finish milling the four squares and square holes, leaving a single-sided semi-finishing allowance of 1mm to prepare for the final finishing;

[0040] S7, perform liquid nitrogen low-temperature aging treatment, place liquid nitrogen at minus 40°C for 36 hours to further stabilize the size;

[0041] S8, finish turning each outer circle, finish milling the four squares and square holes, leaving a single-sided semi-finishing allowance of 0.5mm to prepare for the final finishing;

[0042] S9, grinding the reference surface to a flatness of 0.005 and obtaining the processing technology benchmark;

[0043] S10. Using the grinding reference surface as a reference, the five-axis machining center worktable 1 processes the square and square holes and the holes in relative positions to obtain the accuracy required by the drawing for each hole.

[0044] The process sequence is: blanking → rough turning of the outer circle, rough milling of the square and inner cavity allowance → high temperature aging treatment → semi-finishing turning of the outer circle and semi-finishing milling of the square and inner cavity allowance → medium temperature aging treatment → finishing turning of the outer circle and finishing milling of the square and inner cavity → liquid nitrogen low temperature aging treatment → grinding of the reference surface → five-axis machining center to process the square, square holes and relative position holes;

[0045] From the above, we can see that 7075-T651 imported aluminum alloy bars are used. The maximum size of the piece is Φ234×345.5, and the main accuracy requirements are and Each external circle tolerance, cylindricality requirements and related end faces to the external circle The flatness and parallelism of (datum B), datum A, and C require 0.01 and the tolerance of each hole. The whole process adopts turning and milling combination processing, among which the milling process adopts four-axis and five-axis combination processing. The process is rough turning, rough milling, semi-finishing turning, semi-finishing milling, and finally grinding the datum surface and tooling positioning surface, and finally finishing turning and finishing milling. The processing plan is guaranteed. and The position accuracy of each outer circle relative to each reference surface and the mutual position accuracy are processed by a five-axis machining center, with three medium and low temperature aging treatments interspersed in between, specifically, stress relief aging treatment is carried out after rough turning, medium temperature aging treatment is carried out after semi-finishing, and liquid nitrogen low-temperature aging treatment is carried out after semi-finishing and before finishing. In the finishing, the reference surface is first ground, and then special tooling is designed in combination with special bonding technology to greatly increase the milling and clamping stability of the part, and cleverly solves the problem of large deformation and vibration of the overall processing and clamping of complex tower-shaped parts. When the present invention is used for pagoda-shaped parts with small and medium batches, difficult clamping and alignment, large material removal, and large deformation and vibration, the processing and clamping method and heat treatment process are unique, the tooling is simple (turning and milling combination, four-axis machining center combined with five-axis machining technology), the labor intensity is reduced, and the processing quality and efficiency are improved.

[0046] The high-strength 7075-T651 aluminum alloy bar is selected to ensure the basic performance of the parts. Most of the material excess is removed through rough turning, and the machining allowance is gradually reduced in stages, which is both efficient and reduces the risk of thermal deformation in subsequent finishing.

[0047] Through high-temperature aging, medium-temperature aging and liquid nitrogen low-temperature aging treatment, the internal stress of the material is released step by step, which significantly improves the stability of the part size, reduces the deformation problem during the processing, and ensures the processing accuracy and long-term stability of the finished product; by gradually reducing the processing allowance, the final finishing requirements are met, and the reference surface is ground to a very high flatness, which provides an accurate processing reference for the five-axis machining center, ensuring high-precision processing of key parts such as square and square holes;

[0048] Embodiment 2: As shown in the attached Figure 2 As shown: This embodiment is basically the same as the previous embodiment, except that a fixture 8, a secondary pressure plate support column 3 and a main pressure plate support column 11 are installed on the upper surface of the five-axis machining center worktable 1, a main pressure plate 10 is installed on the top wall of the main pressure plate support column 11, a secondary pressure plate 4 is installed on the top wall of the secondary pressure plate support column 3, and clamping screws 9 are installed on the surfaces of the main pressure plate 10 and the secondary pressure plate 4;

[0049] A viscose substrate support block 2 is also installed on the upper surface of the five-axis machining center workbench 1 . A viscose substrate 5 is supported on the upper surface of the viscose substrate support block 2 . The viscose substrate 5 is located below the secondary pressing plate 4 .

[0050] As can be seen from the above, firstly, the workpiece 6 to be processed is pressed by the fixture 8 in combination with the main pressure plate 10, the clamping bolt 9 and the pressure plate support column 11 on the workbench 1 of the five-axis machining center, and then the side door of the part 6 to be processed is firmly bonded by the adhesive substrate 5 in combination with the secondary pressure plate 4 and the secondary pressure plate support column 3 at the appropriate position of the part 6 to be processed to prevent the part from shaking under force, and the foam filler is added to the middle gap of the part 6 to be processed. Under the action of the foam filler and the auxiliary adhesive, the deformation of the thin-walled part is effectively reduced, and the precision of the processed part is ensured;

[0051] When clamping the workpiece, first use the integral combined secondary clamp, secondary clamp bolts and clamp support column to position the overall center clamp on the workbench of the five-axis machining center, and then use the main clamp bolts and auxiliary adhesive on the overall center clamp to prevent the parts from being deformed by pressure. When bonding, strictly follow the following order:

[0052] 1. Straighten the workpiece (place a shim on the workpiece to increase the weight to prevent the workpiece from being unstable during the straightening process);

[0053] 2. You can stroke the workpiece with your hand and apply glue (502) to fix the position (502 glue has a faster bonding speed);

[0054] 3. For AB glue, intermittent and symmetrical glue dispensing is adopted, the glue dispensing area is T3*10*4, the spacing is 50mm, and the glue drying time is 20 minutes (the glue is milky white in solid state, and blowing can speed up the glue drying speed); the glue removal process adopts blowing processing, the milling contour is left with 0.2mm, and the glue remover is sprayed. After five minutes, it is blown clean with an air gun, and the workpiece is gently lifted with a thin sheet tool;

[0055] 4. After degumming, gently wipe the workpiece with alcohol cotton yarn (if there are glue blocks remaining on the surface of the workpiece, you can spray appropriate degumming agent again. Pay attention to safety during the process, as the degumming agent is slightly corrosive to the skin).

[0056] The combined use of the fixture, primary and secondary pressure plate support columns 11, the secondary pressure plate 4, the primary pressure plate 10 and the adhesive substrate support block 2 ensures stable positioning of the workpiece, and the fixation by the adhesive substrate 5 and the auxiliary adhesive 7 effectively prevents the vibration and deformation of the thin-walled parts during processing, greatly improving the processing stability and accuracy. The foam filler further reduces the influence of the cutting force on the thin-walled structure during processing. Combined with the bonding technology, the workpiece can be processed in a natural state, which minimizes deformation and ensures dimensional accuracy and surface quality.

[0057] For the overall processing of complex aluminum alloy pagoda-shaped parts, bonding clamping combined with filling support can keep the workpiece in a natural state with minimal deformation and maximum dimensional stability.

[0058] The embodiments of the present invention are provided for the purpose of illustration and description. Although the embodiments of the present invention have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations of the present invention. Ordinary technicians in this field can change, modify, replace and deform the above embodiments within the scope of the present invention.

[0059] In the description of the present invention, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. "Multiple" means two or more, unless otherwise clearly and specifically defined.

[0060] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0061] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0062] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are contradictory.

[0063] In the drawings of the embodiments disclosed in the present invention, only the structures involved in the embodiments disclosed in the present invention are involved, and other structures can refer to the general design. In the absence of conflict, the same embodiment and different embodiments of the present invention can be combined with each other.

[0064] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for integrally processing a complex aluminum alloy pagoda-shaped part, characterized in that: The following steps are involved: S1. Use 7075-T651 imported aluminum alloy bars; S2, Rough Turning Each outer circle; S3, high temperature aging treatment; S4, first semi-finish turning of all outer circles, rough milling of four squares and square holes; S5, performing medium temperature aging treatment; S6, semi-finish turning each outer circle again, semi-finish milling the four squares and each square hole; S7, performing liquid nitrogen low temperature aging treatment; S8, precision turning of all outer circles, precision milling of four squares and square holes; S9, grinding the reference surface to a flatness of 0.005 and obtaining the processing technology benchmark; S10. Using the grinding reference surface as the reference, the five-axis machining center processes the square and square holes, and the holes in relative positions to obtain the accuracy required by the drawing for each hole.

2. A method for integrally processing a complex aluminum alloy pagoda-shaped part as claimed in claim 1, characterized in that: The upper surface of the five-axis machining center workbench (1) is installed with a tooling fixture (8), a secondary pressure plate support column (3) and a main pressure plate support column (11); the main pressure plate (10) is installed on the top wall of the main pressure plate support column (11); the secondary pressure plate (4) is installed on the top wall of the secondary pressure plate support column (3); clamping screws (9) are installed on the surfaces of the main pressure plate (10) and the secondary pressure plate (4); the bottom end of the clamping screw (9) is connected to the positioning groove of the five-axis machining center workbench (1); A viscose substrate support block (2) is also installed on the upper surface of the five-axis machining center workbench (1), and a viscose substrate (5) is supported on the upper surface of the viscose substrate support block (2), wherein the viscose substrate (5) is located below the secondary pressure plate (4).

3. A method for integrally processing a complex aluminum alloy pagoda-shaped part as claimed in claim 2, characterized in that: The S2 medium rough turning leaves a single-sided semi-finishing allowance of 2-3 mm.

4. A method for integrally processing a complex aluminum alloy pagoda-shaped part as claimed in claim 3, characterized in that: In the first semi-finishing turning in S4, a single-sided semi-finishing allowance of 1-2 mm is left.

5. A method for integrally processing a complex aluminum alloy pagoda-shaped part as claimed in claim 4, characterized in that: The medium-temperature aging treatment in S5 is performed by heating to 220° C.-180° C. and keeping the temperature for 12 hours.

6. A method for integrally processing a complex aluminum alloy pagoda-shaped part as claimed in claim 5, characterized in that: The second semi-finishing turning in S6 leaves a single-sided semi-finishing allowance of 1 mm.

7. A method for integrally processing a complex aluminum alloy pagoda-shaped part as claimed in claim 6, characterized in that: The S7 low temperature aging treatment is placed in liquid nitrogen at -40°C for 36 hours.

8. A method for integrally processing a complex aluminum alloy pagoda-shaped part as claimed in claim 7, characterized in that: In the S8, a single-sided semi-finishing allowance of 0.5 mm is left.

Citation Information

Patent Citations

  • Aluminum alloy middle frame thin-wall part machining method

    CN115805417A

  • Machining process of aluminum alloy thin-wall sealing guide cylinder

    CN116922003A

  • Thin-wall complex aluminum alloy part machining method

    CN117047420A

  • Base part production isolated plant

    CN205111272U

  • Tooling structure with upper pressing and lower gluing functions

    CN220286149U