Surface treatment GSP technology after Diffuser sand blasting

Through the Diffuser surface treatment GSP process after sandblasting, white corundum and spherical sand materials are used to remove unstable tip particles and residual films in CVD equipment, solving the dust pollution caused by plasma, and improving the structural strength and wear resistance of the equipment surface sex.

CN118875976APending Publication Date: 2024-11-01ANHUI YINGYOU OPTOELECTRONICS TECH CO LTD

Patent Information

Application Number
CN202411256137.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

During the existing CVD process, gas dissociation forms plasma, resulting in dust particles contamination, affecting the finished product efficiency and use of liquid crystal panels and equipment.

Method used

The surface treatment GSP process after Diffuser sandblasting is adopted. The unstable tip particles and residual film in the deep valley area are removed by sandblasting of white corundum and 600-800nm ​​spherical sand material, so as to improve the structural strength of the AL layer surface and clean the residual substances by ultrasonic wave.

Benefits of technology

It significantly reduces the probability of dust particles falling, improves the structural strength and wear resistance of the surface layer, and ensures the finished product quality of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118875976A_ABST
    Figure CN118875976A_ABST
Patent Text Reader

Abstract

The invention discloses a surface treatment GSP process after Diffuser sand blasting, which comprises a Diffuser body and a conventional white corundum sand material, and comprises the following process steps: fixing the Diffuser body and a sand blasting gun nozzle, and enabling the Diffuser body and the sand blasting gun nozzle to be in a horizontal and vertical state; filling white corundum, and starting a sand blasting machine to perform first sand blasting; the Diffuser body is turned over to be subjected to sand blasting for the second time; replacing the white corundum with a spherical sand material, and carrying out third sand blasting; the Diffuser body is turned over again, and fourth sand blasting is carried out; cleaning the surface of the Diffuser body and testing the surface of the Diffuser body; sand blasting materials are replaced after the first-time white corundum sand blasting is carried out on the front face and the back face of the Diffuser body, and sand blasting is carried out on the front face and the back face again; a large number of unstable tip particles generated on the surface and residual films in a deep valley area after the surface of the Diffuser body is impacted by the first-time white corundum sand blasting are greatly removed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of CVD diffuser surface treatment, in particular to a GSP process for diffuser surface treatment after sandblasting. Background Art

[0002] In the manufacturing process of liquid crystal display panels, some functional films need to be deposited on the surface of glass substrates using chemical vapor deposition (CVD) technology. The CVD equipment uses a gas diffuser to deposit the film, but the existing GSP process of surface treatment after sandblasting by the diffuser has some shortcomings, such as:

[0003] In the existing CVD process, in addition to some specific gases, electricity is also required in the reaction chamber to dissociate the gas to form plasma. If dust particles are formed by peeling during the reaction, they will contaminate the LCD panel glass and equipment, which may affect the finished product efficiency and use of the LCD panel glass and equipment.

[0004] Therefore, we proposed a GSP process for surface treatment after Diffuser sandblasting to solve the above problems. Summary of the invention

[0005] The purpose of the present invention is to provide a GSP process for surface treatment after diffuser sandblasting to solve the problem that the existing CVD process on the market, in addition to some specific gases, needs to be powered on in the reaction chamber to dissociate the gas to form plasma. If dust particles fall off during the reaction, they will contaminate the liquid crystal panel glass and equipment; thus, they may affect the finished product efficiency and usage of the liquid crystal panel glass and equipment.

[0006] To achieve the above object, the present invention provides the following technical solution: a Diffuser post-sandblasting surface treatment GSP process, comprising a Diffuser body and conventional white corundum abrasive material, and comprising the following process steps:

[0007] S1. Install the hanging screws in the two side screw holes of the Diffuser body after surface grinding, and then connect the screws to the hanger. Use the crane to vertically erect the Diffuser body and install it on the sandblasting hanging fixture, keeping the front facing the sandblasting gun nozzle, so that the Diffuser body and the sandblasting gun nozzle are in a horizontal and vertical state;

[0008] S2. Add the corresponding white corundum blasting material into the sandblasting tank, set the pressure value during sandblasting, and adjust the sandblasting distance between the spray gun nozzle and the diffuser body;

[0009] S3. Set the corresponding angle between the sandblasting gun nozzle and the product to 90 degrees from left to right, set the gun speed and the upper and lower interval distances, and start the sandblasting machine for the first sandblasting;

[0010] After setting the gun speed and upper and lower intermittent distances, you can first test spray the sample, and then adjust the gun speed and the spacing value of the upper and lower intermittent distances according to the sandblasting effect of the sample;

[0011] S4. After the first sandblasting is completed, remove the Diffuser body from the sandblasting fixture, turn it over, make the back side correspond to the spray gun nozzle and install it, keep the sandblasting nozzle angle, sandblasting pressure value, sandblasting distance, upper and lower interruption distance unchanged, and perform the second sandblasting;

[0012] S5. At this time, the sand material in the sandblasting tank is replaced with 600-800nm ​​spherical sand material, and the sandblasting nozzle angle, sandblasting pressure value, sandblasting distance and upper and lower interruption distance are kept unchanged, and then the third sandblasting is carried out;

[0013] S6. After the third sandblasting is completed, remove the Diffuser body from the sandblasting fixture, turn it over, keep the sandblasting nozzle angle, sandblasting pressure value, sandblasting distance, and upper and lower interruption distance unchanged, and perform the fourth sandblasting;

[0014] S7, removing the Diffuser body from the sandblasting jig, cleaning the surface of the Diffuser body, and then inspecting the surface thereof, thereby completing the GSP process;

[0015] The diffuser body is a gas diffuser for a chemical vapor deposition (CVD) process, and the diffuser body is made of aluminum.

[0016] By replacing the sandblasting material after the first white corundum sandblasting on the front and back sides of the Diffuser body, and sandblasting the front and back sides again, a large number of unstable tip particles and residual film in the deep valley area generated on the surface of the Diffuser body after the first white corundum sandblasting can be removed, which greatly reduces the probability of the finished product falling during the operation of the CVD equipment.

[0017] As a preferred technical solution of the present invention, the diffuser body adopts the GSP process after shaping, film removal, grinding and the conventional white corundum sand blasting process. The principle of the GSP process is to use a high-speed particle flow of 600-800nm ​​to impact the AL layer surface of the diffuser body to remove unstable tip particles caused by sandblasting, thereby improving the loose structural properties of the AL layer surface, thereby improving the structural strength of the surface layer, and removing a large amount of tip particles and residual film in the deep valley area.

[0018] By adopting the above technical solution, after the surface of the AL layer is washed by high-speed particles again, the surface particles except the tip particles and residual film in the deep valley area will be dispersed by the high-speed particles, so that no residual film except the tip particles and residual film in the deep valley area will remain on the surface of the AL layer.

[0019] As the preferred technical solution of the present invention, after the diffuser body is sandblasted with white corundum, a large number of tip particles and deep valley residual film will be formed on the surface of the AL layer. The tip particles are easily fluorinated and fall off (peeling) during the operation of the CVD equipment to form dust particles (particles), which is particularly obvious in the first piece (CC1) after the chamber is cleaned; the residual film at the bottom of the deep valley is not easy to remove (clean), resulting in residual film falling dust particles (peelingparticles), which is particularly obvious in the second piece (CC2) after the chamber is cleaned.

[0020] As a preferred technical solution of the present invention, the tip particles and the residual film in the deep valley are observed under the microscopic state of the surface of the AL layer after white corundum sandblasting. When the texture of the surface of the AL layer becomes clear, the surface becomes more rounded and full, a large number of tips disappear, and the residual film in the deep valley area is completely removed under the microscopic state, the subsequent anode cleaning process is carried out.

[0021] The adoption of the above technical solution makes it more convenient to observe the tip particles and the residual film in the deep valley when the Diffuser body is taken out in a microscopic state, thereby making the surface of the AL layer smoother.

[0022] As a preferred technical solution of the present invention, the material for sandblasting the Diffuser body is white corundum, and the grain number grade of the white corundum is 220#. The white corundum has a dense texture, high hardness, and insulation, and the grains form sharp corners;

[0023] When using white corundum as a sandblasting material, a magnet is needed to remove iron from the white corundum material. The pressure value during sandblasting is 0.25MPa, and the sandblasting distance is 600mm.

[0024] The above technical solution can ensure that when the sandblasting gun nozzle performs sandblasting on the diffuser body, the white corundum or spherical sand material will not damage the surface of the diffuser body due to excessive pressure or too close sandblasting distance.

[0025] As a preferred technical solution of the present invention, the sandblasting gun nozzle has a gun travel speed of 10 mm / s, an upper and lower discontinuity distance of 4 mm, and a filtering mechanism can be provided at the feed inlet of the sandblasting gun nozzle to filter out impurities when feeding.

[0026] The above technical solution enables the sandblasting gun nozzle to filter the sand material through the filtering mechanism when spraying white corundum or spherical sand material, thereby preventing impurities from being sprayed on the surface of the diffuser body, thereby increasing the protectiveness of the equipment.

[0027] As the preferred technical solution of the present invention, the 600-800nm ​​spherical sand material is a kind of corundum (SiC), which is a kind of corundum, an inorganic non-metallic material, a hexagonal crystal, a specific gravity of 3.20-3.25, and a microhardness of 2840-3320kg / mm 2 .

[0028] The above technical solution can remove unstable tip particles caused by sandblasting on the surface of the Diffuser body during the third and fourth sandblasting, improve the loose structural properties of the AL layer surface, and thus improve the structural strength of the surface layer.

[0029] As a preferred technical solution of the present invention, when detecting the Diffuser body, the surface of the Diffuser body can be detected by a roughness probe, so as to measure the roughness of the surface of the Diffuser body.

[0030] By adopting the above technical solution, when detecting the surface of the Diffuser body, the roughness of the surface can be detected by the roughness probe, thereby making it more convenient to detect the surface of the Diffuser body.

[0031] As a preferred technical solution of the present invention, when detecting the arithmetic mean of the contour deviation within the sampling length of the Diffuser body, the calculation is performed according to the following formula:

[0032] The above technical solution can be used to calculate the arithmetic mean of the contour deviation within the sampling length of the Diffuser body through a formula when detecting the arithmetic mean of the contour deviation within the sampling length of the Diffuser body, thereby making it more convenient to calculate the arithmetic mean of the contour deviation within the sampling length of the Diffuser body.

[0033] As a preferred technical solution of the present invention, the diffuser body is made of 6061 series aluminum, and 6061 series aluminum is a magnesium-aluminum alloy material, which has good plasticity, corrosion resistance and high toughness, and is not easy to deform and oxidize after processing;

[0034] When cleaning the surface of the Diffuser body, an ultrasonic device may be used to clean the surface, so that the white corundum or spherical sand material remaining on the surface of the Diffuser body is vibrated by the ultrasonic wave, thereby causing the remaining material to fall off.

[0035] The adoption of the above technical solution can increase the strength of the Diffuser body itself, so that the Diffuser body is not easily deformed after processing, thereby ensuring the wear resistance of its surface after processing.

[0036] Compared with the prior art, the present invention has the following beneficial effects: by replacing the blasting material after the first white corundum blasting on the front and back sides of the diffuser body, and blasting the front and back sides again, a large number of unstable tip particles and residual film in the deep valley area generated on the surface of the diffuser body after the first white corundum blasting impacts the surface of the diffuser body can be removed in large quantities, thereby greatly reducing the probability of the finished product falling during the operation of the CVD equipment;

[0037] Furthermore, by adjusting the blasting pressure and blasting distance, the sandblasting nozzle can prevent the white corundum or spherical sand material from damaging the surface of the Diffuser body due to excessive pressure or too close blasting distance when the Diffuser body is blasted.

[0038] Furthermore, by making the Diffuser body of magnesium-aluminum alloy material, the strength of the Diffuser body itself can be increased, making the Diffuser body less likely to deform after processing, thereby ensuring the wear resistance of its surface after processing. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a schematic diagram of the process structure of the present invention;

[0040] Figure 2 It is a detailed process structure schematic diagram of the present invention;

[0041] Figure 3 A schematic diagram of roughness detection of the present invention;

[0042] Figure 4 It is a schematic diagram for calculating the arithmetic mean deviation value of the profile of the present invention. DETAILED DESCRIPTION

[0043] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0044] Embodiment 1:

[0045] See also Figure 1-4 The present invention provides a technical solution: a Diffuser post-sandblasting surface treatment GSP process, comprising a Diffuser body and conventional white corundum sand material, and comprising the following process steps:

[0046] S1. Install the hanging screws in the two side screw holes of the Diffuser body after surface grinding, and then connect the screws to the hanger. Use the crane to vertically erect the Diffuser body and install it on the sandblasting hanging fixture, keeping the front facing the sandblasting gun nozzle, so that the Diffuser body and the sandblasting gun nozzle are in a horizontal and vertical state;

[0047] S2. Add the corresponding white corundum blasting material into the sandblasting tank, set the pressure value during sandblasting, and adjust the sandblasting distance between the spray gun nozzle and the diffuser body;

[0048] S3. Set the corresponding angle between the sandblasting gun nozzle and the product to 90 degrees from left to right, set the gun speed and the upper and lower interval distances, and start the sandblasting machine for the first sandblasting;

[0049] S4. After the first sandblasting is completed, remove the Diffuser body from the sandblasting fixture, turn it over, make the back side correspond to the spray gun nozzle and install it, keep the sandblasting nozzle angle, sandblasting pressure value, sandblasting distance, upper and lower interruption distance unchanged, and perform the second sandblasting;

[0050] S5. At this time, the sand material in the sandblasting tank is replaced with 600nm spherical sand material, and the sandblasting nozzle angle, sandblasting pressure value, sandblasting distance and upper and lower interruption distance are kept unchanged, and then the third sandblasting is performed;

[0051] S6. After the third sandblasting is completed, remove the Diffuser body from the sandblasting fixture, turn it over, keep the sandblasting nozzle angle, sandblasting pressure value, sandblasting distance, and upper and lower interruption distance unchanged, and perform the fourth sandblasting;

[0052] S7, removing the Diffuser body from the sandblasting jig, cleaning the surface of the Diffuser body, and then inspecting the surface thereof, thereby completing the GSP process;

[0053] When detecting the surface of the diffuser body, the roughness probe can be moved by the extension mechanism, so that the roughness probe always outputs the same height state;

[0054] The Diffuser body is a gas diffuser for chemical vapor deposition (CVD) process, and the Diffuser body is made of aluminum;

[0055] The diffuser body is subjected to the GSP process after shaping, film removal, grinding and the conventional white corundum sand blasting process. The GSP process principle is to use a 600 high-speed particle flow to impact the AL layer surface of the diffuser body to remove unstable tip particles caused by sand blasting, thereby improving the loose structural properties of the AL layer surface, thereby improving the structural strength of the surface layer, and removing a large amount of tip particles and residual film in the deep valley area;

[0056] After the diffuser body is blasted with white corundum, a large number of tip particles and deep valley residual film will form on the surface of the AL layer. The tip particles are easy to fluorinate and fall off (peeling) during the operation of the CVD equipment to form dust particles (particles), which is particularly obvious in the first piece (CC1) after the chamber is cleaned; the residual film at the bottom of the deep valley is not easy to remove (clean), resulting in residual film falling dust particles (peelingparticles), which is particularly obvious in the second piece (CC2) after the chamber is cleaned;

[0057] After white corundum sandblasting, the tip particles and residual film in the deep valley are observed under the microscopic state of the AL layer surface. When the AL layer surface becomes clear in texture, the surface becomes more rounded and full, a large number of tips disappear, and the residual film in the deep valley area is completely removed, the subsequent anode cleaning process is carried out.

[0058] The material used for sandblasting the Diffuser body is white corundum, and the grain number grade of white corundum is 220#. White corundum has a dense texture, high hardness, and insulation, and the grains are in a sharp angle. When using white corundum as a sandblasting material, a practical magnet is needed to remove iron from the white corundum material, and the pressure value during sandblasting is 0.25MPa, and the sandblasting distance is 600mm.

[0059] The speed of the sandblasting gun is 10 mm / s, the upper and lower intervals are 4 mm, and a filter mechanism can be set at the feed port to filter out impurities when the sandblasting gun is feeding; 600 spherical sand material is a kind of corundum (SiC), which is a kind of corundum, an inorganic non-metallic material, a hexagonal crystal, with a specific gravity of 3.20 and a microhardness of 2840 / mm 2 ;

[0060] like Figure 3 As shown, when inspecting the Diffuser body, the surface of the Diffuser body can be inspected by a roughness probe, so that the roughness of the surface of the Diffuser body can be measured;

[0061] like Figure 4 As shown: When detecting the arithmetic mean of the contour deviation within the sampling length of the Diffuser body, the calculation is performed according to the following formula:

[0062] The tip is a dust particle formed by fluorination and peeling;

[0063] Moreover, the residual film on the bottom is not easy to clean, resulting in peeling particles from the residual film.

[0064] The diffuser body is made of 6061 series aluminum, which is a magnesium-aluminum alloy material with good plasticity, corrosion resistance and high toughness, and is not easy to deform and oxidize after processing;

[0065] When performing the GSP process on a Diffuser body with a relatively smooth surface or soft material, 600 spherical sand materials are used, which can reduce the wear of the spherical sand materials on the Diffuser body, and will not affect the loose structural properties of the AL layer surface, and can improve the structural strength of the surface layer, and remove the tip particles and residual film in the deep valley area; thus, the unstable tip particles and residual film in the deep valley area generated on the surface after the spherical sand material sandblasting impacts the Diffuser body can be removed. Compared with the conventional white corundum sandblasting process, the unstable tip particles and residual film can be better removed, and the white corundum sandblasting can be prevented from sticking to the Diffuser body to form discolored substances, making the surface of the Diffuser body smoother, and increasing the efficiency and protection of the process in processing the Diffuser body;

[0066] Embodiment 2:

[0067] The present embodiment differs from the first embodiment in that: a GSP process for surface treatment after sandblasting of a diffuser comprises a diffuser body and conventional white corundum sand material, and comprises the following process steps:

[0068] S1. Install the hanging screws in the two side screw holes of the Diffuser body after surface grinding, and then connect the screws to the hanger. Use the crane to vertically erect the Diffuser body and install it on the sandblasting hanging fixture, keeping the front facing the sandblasting gun nozzle, so that the Diffuser body and the sandblasting gun nozzle are in a horizontal and vertical state;

[0069] S2. Add the corresponding white corundum blasting material into the sandblasting tank, set the pressure value during sandblasting, and adjust the sandblasting distance between the spray gun nozzle and the diffuser body;

[0070] S3. Set the corresponding angle between the sandblasting gun nozzle and the product to 90 degrees from left to right, set the gun speed and the upper and lower interval distances, and start the sandblasting machine for the first sandblasting;

[0071] S4. After the first sandblasting is completed, remove the Diffuser body from the sandblasting fixture, turn it over, make the back side correspond to the spray gun nozzle and install it, keep the sandblasting nozzle angle, sandblasting pressure value, sandblasting distance, upper and lower interruption distance unchanged, and perform the second sandblasting;

[0072] S5. At this time, the sand material in the sandblasting tank is replaced with 800nm ​​spherical sand material, and the sandblasting nozzle angle, sandblasting pressure value, sandblasting distance and upper and lower interruption distance are kept unchanged, and then the third sandblasting is performed;

[0073] S6. After the third sandblasting is completed, remove the Diffuser body from the sandblasting fixture, turn it over, keep the sandblasting nozzle angle, sandblasting pressure value, sandblasting distance, and upper and lower interruption distance unchanged, and perform the fourth sandblasting;

[0074] S7, removing the Diffuser body from the sandblasting jig, cleaning the surface of the Diffuser body, and then inspecting the surface thereof, thereby completing the GSP process;

[0075] When detecting the surface of the diffuser body, the roughness probe can be moved by the extension mechanism, so that the roughness probe always outputs the same height state;

[0076] The diffuser body is subjected to the GSP process after shaping, film removal, grinding and the conventional white corundum sand blasting process. The GSP process principle is to use a high-speed particle flow of 800 to impact the AL layer surface of the diffuser body to remove unstable tip particles caused by sand blasting, thereby improving the loose structural properties of the AL layer surface, thereby improving the structural strength of the surface layer, and removing a large amount of tip particles and residual film in the deep valley area;

[0077] The Diffuser body is a gas diffuser for chemical vapor deposition (CVD) process, and the Diffuser body is made of aluminum;

[0078] The material for sandblasting the Diffuser body is white corundum, and the grain number grade of white corundum is 220#, and the pressure value during sandblasting is 0.25MPa, and the sandblasting distance is 600mm; the speed of the sandblasting gun nozzle is 10mm / s, the upper and lower discontinuity distance is 4mm, and when the sandblasting gun nozzle is feeding, a filtering mechanism can be set at the feeding port to filter out its impurities;

[0079] 800nm ​​spherical sand material is a kind of corundum (SiC), which is a kind of corundum. It is an inorganic non-metallic material with a hexagonal crystal, a specific gravity of 3.25, and a microhardness of 320kg / mm 2 ;

[0080] By adopting 800nm ​​spherical sand material, the GSP process can better sandblast the surface of the Diffuser body when sandblasting the Diffuser body with harder material and more residual film, and can more effectively improve the loose structural properties of the AL layer surface, thereby improving the structural strength of the surface layer, and remove a large amount of residual film in the tip particles and deep valley areas, thereby increasing the structural strength of the AL layer surface, and preventing the tip particles and residual film from affecting the surface of the Diffuser body.

[0081] Thereby completing a series of tasks, the contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.

[0082] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A GSP process for surface treatment after diffuser sandblasting. It is characterized in that It includes a Diffuser body and conventional white corundum abrasive material, and includes the following process steps: S1. Install the hanging screws in the two side screw holes of the Diffuser body after surface grinding, and then connect the screws to the hanger. Use the crane to vertically erect the Diffuser body and install it on the sandblasting hanging fixture, keeping the front facing the sandblasting gun nozzle, so that the Diffuser body and the sandblasting gun nozzle are in a horizontal and vertical state; S2. Add the corresponding white corundum blasting material into the sandblasting tank, set the pressure value during sandblasting, and adjust the sandblasting distance between the spray gun nozzle and the diffuser body; S3. Set the corresponding angle between the sandblasting gun nozzle and the product to 90 degrees from left to right, set the gun speed and the upper and lower interval distances, and start the sandblasting machine for the first sandblasting; S4. After the first sandblasting is completed, remove the Diffuser body from the sandblasting fixture, turn it over, make the back side correspond to the spray gun nozzle and install it, keep the sandblasting nozzle angle, sandblasting pressure value, sandblasting distance, upper and lower interruption distance unchanged, and perform the second sandblasting; S5. At this time, the sand material in the sandblasting tank is replaced with 600-800nm ​​spherical sand material, and the sandblasting nozzle angle, sandblasting pressure value, sandblasting distance and upper and lower interruption distance are kept unchanged, and then the third sandblasting is carried out; S6. After the third sandblasting is completed, remove the Diffuser body from the sandblasting fixture, turn it over, keep the sandblasting nozzle angle, sandblasting pressure value, sandblasting distance, and upper and lower interruption distance unchanged, and perform the fourth sandblasting; S7, removing the Diffuser body from the sandblasting jig, cleaning the surface of the Diffuser body, and then inspecting the surface thereof, thereby completing the GSP process; The diffuser body is a gas diffuser for a chemical vapor deposition (CVD) process, and the diffuser body is made of aluminum.

2. The Diffuser post-sandblasting surface treatment GSP process according to claim 1, It is characterized in that The diffuser body is subjected to the GSP process after shaping, film removal, grinding and the conventional white corundum sand blasting process. The GSP process principle is to use a high-speed particle flow of 600-800nm ​​to impact the AL layer surface of the diffuser body to remove unstable tip particles caused by sandblasting, thereby improving the loose structural properties of the AL layer surface, thereby improving the structural strength of the surface layer, and removing a large amount of tip particles and residual film in the deep valley area.

3. The GSP process for surface treatment after Diffuser sandblasting according to claim 1, It is characterized in that After the diffuser body is blasted with white corundum, a large number of tip particles and deep valley residual film will form on the surface of the AL layer. The tip particles are easy to fluorinate and fall off (peeling) during the operation of the CVD equipment to form dust particles (particles), which is particularly obvious in the first piece (CC1) after the chamber is cleaned; The residual film at the bottom of the valley is not easy to remove (clean), resulting in residual film falling dust particles (peeling particle), which is particularly obvious in the second piece (CC2) after the chamber is cleaned.

4. The GSP process for surface treatment after Diffuser sandblasting according to claim 1, It is characterized in that After white corundum sandblasting, the tip particles and residual film in the deep valley are observed under the microscopic state of the AL layer surface. When the AL layer surface becomes clear in texture, the surface becomes more rounded and full, a large number of tips disappear, and the residual film in the deep valley area is completely removed, the subsequent anode cleaning process is carried out.

5. The Diffuser post-sandblasting surface treatment GSP process according to claim 1, It is characterized in that The material used for sandblasting the Diffuser body is white corundum, and the grain number grade of white corundum is 220#, and the pressure value during sandblasting is 0.25MPa, and the sandblasting distance is 600mm. White corundum has a dense texture, high hardness, and insulation, and the grains form sharp corners; When white corundum is used as a sandblasting material, a magnet is needed to remove iron from the white corundum material.

6. The Diffuser post-sandblasting surface treatment GSP process according to claim 1, It is characterized in that The speed of the sandblasting gun nozzle is 10 mm / s, the upper and lower interval distance is 4 mm, and when the sandblasting gun nozzle is feeding, a filtering mechanism can be set at the feeding port to filter out impurities.

7. The Diffuser post-sandblasting surface treatment GSP process according to claim 1, It is characterized in that 600-800nm ​​spherical sand material is a kind of corundum (SiC), which is a kind of corundum. It is an inorganic non-metallic material with a hexagonal crystal, a specific gravity of 3.20-3.25, and a microhardness of 2840-3320kg / mm 2 .

8. The Diffuser post-sandblasting surface treatment GSP process according to claim 1, It is characterized in that When inspecting the Diffuser body, the surface of the Diffuser body can be inspected by a roughness probe, thereby being able to measure the roughness of the surface of the Diffuser body.

9. The GSP process for surface treatment after Diffuser sandblasting according to claim 1, It is characterized in that When detecting the arithmetic mean of the contour deviation within the sampling length of the diffuser body, the calculation is performed according to the following formula:

10. The Diffuser post-sandblasting surface treatment GSP process according to claim 1, It is characterized in that The diffuser body is made of 6061 series aluminum, which is a magnesium-aluminum alloy material with good plasticity, corrosion resistance and high toughness, and is not easily deformed or oxidized after processing.

Citation Information

Patent Citations

  • Surface pretreatment process for diamond-like carbon coated workpiece

    CN103952664A

  • Cutter surface plasma vacuum coating pretreatment process

    CN109182963A

  • In-hole sand blasting method for application material equipment diffuser

    CN115008348A

Cited By

  • Sand blasting precision detection method for wearable watch bottom shell

    CN119407695A