Preparation method of flame-retardant reconstituted bamboo capable of preventing loss of flame retardant
By impregnating reconstituted bamboo units with flame retardants and resin through mechanical extrusion, the problem of flame retardant loss during the preparation of reconstituted bamboo was solved, thereby improving the flame retardant effect and enabling the clean utilization of the adhesive, thus meeting the flame retardant requirements of building components.
Patent Information
- Application Number
- CN202411161133.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-01
AI Technical Summary
In existing technologies, flame retardants are easily lost during the preparation of reconstituted bamboo, resulting in reduced flame retardant effect and adhesive contamination, which affects recycling and bonding quality.
By mechanically extruding the reconstituted bamboo units, the flame retardant and resin are impregnated during the mechanical pressure release process, reducing the residence time of the flame retardant in the water-soluble flame retardant and resin, and achieving uniform penetration of the flame retardant and resin in the reconstituted bamboo units.
It significantly reduces the loss rate of flame retardants, improves the flame retardant effect, avoids adhesive contamination, improves bonding quality, and meets the flame retardant performance requirements of building components.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bamboo material processing, and in particular to a method for preparing flame-retardant reconstituted bamboo capable of preventing the loss of flame retardants. Background Art
[0002] Recombined bamboo is a new type of bamboo-based composite material made by bamboo materials through decomposition and directional reorganization. Due to its excellent physical and mechanical properties, it has been widely used in indoor and outdoor floors, furniture, structural buildings, exterior wall panels and other fields. The national standard requires that the flame retardant performance of building components must reach B1 level or above. However, recombined bamboo is a composite material composed of natural organic polymers and resins (mostly phenolic resins). It is easy to cause fire under the influence of external heat sources or fire sources, and cannot meet the standard requirements, which greatly limits the promotion of recombined bamboo in the construction field.
[0003] The bamboo material is prepared into reconstituted bamboo units after being decomposed, and then the reconstituted bamboo is obtained after being impregnated with glue and hot pressed. The flame retardant treatment of reconstituted bamboo is mainly achieved by applying flame retardants during the preparation process. The prior art basically involves impregnating the flame retardant solution or suspension into the reconstituted bamboo unit under normal pressure or negative pressure before impregnation, or preparing flame retardant phenolic resin by physical blending or chemical modification, and then preparing flame retardant reconstituted bamboo. Water-soluble flame retardants such as ammonium phosphate salts, ammonium sulfate salts, boron compounds and other compounds have the advantages of good water solubility, high flame retardant efficiency, and low price. They are currently commonly used flame retardants in the field of wood and bamboo flame retardancy. From the perspective of the preparation process, the reconstituted bamboo unit is treated with a flame retardant solution, so that the flame retardant components can be evenly penetrated into the cell cavity and cell wall of the bamboo material, and will directly act on the flammable bamboo material itself during combustion, achieving a highly efficient flame retardant effect.
[0004] However, when applying flame retardants, the reconstructed bamboo units need to be placed in a pit-type dipping tank for dipping treatment first, and then taken out and dried after a long time (generally more than 1 hour). The reconstructed bamboo units treated with flame retardant solution also need to apply adhesives by dipping, that is, the flame retardant reconstructed bamboo units are immersed in a resin with a certain solid content for a period of time using a dipping cage or dipping frame, and then taken out and dried. Since commonly used flame retardants are highly water-soluble, during the dipping process, the water-soluble flame retardants in the reconstructed bamboo units will inevitably dissolve into the glue. On the one hand, it will lead to the loss of flame retardants and reduce the flame retardant effect; on the other hand, the loss of flame retardants into the resin will cause problems such as glue contamination and pre-curing, affecting recycling and reducing the quality of bonding.
[0005] Therefore, how to solve the problem of flame retardant loss during the preparation of flame retardant recombinant bamboo is a key issue in the current field of recombinant bamboo technology. Summary of the invention
[0006] In order to solve this technical problem, the present invention provides a method for preparing a flame retardant reconstituted bamboo that prevents the loss of flame retardants, comprising: mechanically extruding reconstituted bamboo units in a flame retardant solution, impregnating the units with flame retardants during the process of releasing the mechanical pressure, and then mechanically extruding the reconstituted bamboo units in a resin solution, allowing the resin to be absorbed into the cell cavity of the reconstituted bamboo units during the process of releasing the mechanical pressure, and then hot pressing the assemblies to obtain the flame retardant reconstituted bamboo.
[0007] The present invention uses a method of mechanically squeezing the recombined bamboo unit and then releasing it, so that the cells inside the recombined bamboo unit are first compressed and deformed, the internal space is compressed, and the internal air is squeezed out. Then, during the release process, the flame retardant or resin is inhaled by negative pressure, thereby reducing the residence time of the recombined bamboo unit in the water-soluble flame retardant and the resin. During this process, only a very small amount of the flame retardant is dissolved, and at the same time, the flame retardant and the resin are quickly and evenly penetrated into the recombinant bamboo unit, thereby significantly improving the loss problem of the flame retardant during the dipping process, improving the flame retardant effect, and avoiding glue liquid pollution.
[0008] In the specific implementation process, the amount of flame retardant added and the amount of glue applied in the reconstructed bamboo unit can be accurately controlled by setting parameters such as compression rate, flame retardant concentration, solid content of glue solution, and number of compressions, thereby achieving precise control of the performance of flame-retardant reconstructed bamboo.
[0009] Preferably, the mechanical pressing is performed using a flat press or a roller press.
[0010] Preferably, the compression rate of the mechanically squeezed reconstructed bamboo unit is 30%-80%.
[0011] More preferably, the compression rate of the mechanically squeezed reconstructed bamboo units is 30%-60%.
[0012] Most preferably, the compression ratio of the mechanically squeezed reconstituted bamboo units when impregnated with the flame retardant and the resin solution is 55%-65%, and most preferably 60%.
[0013] Preferably, the flame retardant solution is circulated for more than 2 times, and most preferably 4 times.
[0014] Preferably, after impregnation with the flame retardant, the reconstituted bamboo unit is dried to a moisture content of 8%-15%.
[0015] Preferably, the reconstituted bamboo unit after the resin adsorption is dried to a moisture content of 8%-15%.
[0016] Preferably, the density of the flame retardant reconstituted bamboo is 0.80-1.30 g / cm 3 .
[0017] Preferably, the flame retardant solution contains at least one of ammonium phosphate, ammonium sulfate, boron compounds and urea; the concentration of the flame retardant solution is 10%-50% (preferably 20%-30%, most preferably 25%).
[0018] Preferably, the solid content of the resin solution is 20%-40%, preferably 25%-35%, most preferably 30%.
[0019] Preferably, the resin includes but is not limited to phenolic resin.
[0020] Preferably, the preparation method of the reconstructed bamboo unit comprises: sawing bamboo into bamboo tubes of a certain length, splitting into bamboo slices, and forming fiberized reconstructed bamboo units through a decomposing machine, and drying to a moisture content of 8%-15%.
[0021] Preferably, the bamboo species of the recombinant bamboo unit is a scattered bamboo species or a clumping bamboo species (including but not limited to Phyllostachys pubescens, Phyllostachys cycads or Phyllostachys longituba).
[0022] Furthermore, the present invention provides flame-retardant reconstituted bamboo prepared by the preparation method of any of the above embodiments.
[0023] Compared with the prior art, the present invention has the following beneficial effects: The present invention proposes a method for preparing flame-retardant reconstituted bamboo based on mechanical extrusion to prevent the loss of flame retardants. Compared with conventional methods, the loss rate of the flame retardant in the preparation method of the present invention is reduced by 60-75% during the flame retardant dipping process. The process of the present invention can significantly reduce the loss of flame retardants during the dipping process, avoid the pollution of the glue solution, and improve the flame retardant performance of the reconstituted bamboo, and has broad application prospects. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] If no specific techniques or conditions are specified in the examples, all are carried out according to conventional methods or the techniques or conditions described in the literature in the field, or according to the product instructions. If no manufacturer is specified for the reagents and instruments used, all are conventional products that can be purchased through regular channels.
[0026] Example 1
[0027] This embodiment provides a flame retardant reconstituted bamboo, and the preparation method thereof is as follows: Prepare a 25% concentration (mass fraction) of ammonium pyrophosphate, ammonium sulfate and urea (mass ratio of 10:5:3) mixed flame retardant solution, soak the bamboo bundles with a moisture content of 10% in the above solution, use the pressing plate of the flat press to compress the bamboo bundles by 60%, then slowly release, cycle twice, then take out to drain the excess solution, and dry to a moisture content of 10%. Prepare a phenolic resin glue with a solid content of 20%, soak the bamboo bundles impregnated with flame retardant in the resin glue, compress and release at a compression rate of 60%, take out to drain, and dry to a moisture content of 10%. Assemble the dried bamboo bundles, and hot press them at a temperature of 150℃ and a pressure of 20MPa for 25 minutes to control the density of the flame retardant recombined bamboo to 1.15g / cm 3 .
[0028] Example 2
[0029] This embodiment provides a flame retardant reconstituted bamboo, and the preparation method is different from that of embodiment 1 only in that: The flame retardant solution was immersed in the solution for 4 cycles.
[0030] Example 3
[0031] This embodiment provides a flame retardant reconstituted bamboo, and the preparation method is different from that of embodiment 1 only in that: Use phenolic resin glue with 30% solid content.
[0032] Example 4
[0033] This embodiment provides a flame retardant reconstituted bamboo, and the preparation method is different from that of embodiment 1 only in that: When dipping in the flame retardant solution, circulate 4 times; use a phenolic resin glue with a solid content of 30%.
[0034] Example 5
[0035] This embodiment provides a flame retardant reconstituted bamboo, and the preparation method is different from that of embodiment 1 only in that: The compression rate is 30% when impregnated with flame retardant solution, and 40% when impregnated with resin glue.
[0036] Example 6
[0037] This embodiment provides a flame retardant reconstituted bamboo, and the preparation method is different from that of embodiment 1 only in that: The compression rate is 30% when impregnated with flame retardant solution, and 60% when impregnated with resin glue.
[0038] Example 7
[0039] This embodiment provides a flame retardant reconstituted bamboo, and the preparation method is different from that of embodiment 1 only in that: The compression rate is 40% when impregnated with flame retardant solution, and 60% when impregnated with resin glue.
[0040] Example 8
[0041] This embodiment provides a flame retardant reconstituted bamboo, and the preparation method is different from that of embodiment 1 only in that: The compression rate is 40% when impregnated with flame retardant solution, and 80% when impregnated with resin glue.
[0042] Example 9
[0043] This embodiment provides a flame retardant reconstituted bamboo, and the preparation method is different from that of embodiment 1 only in that: The compression rate is 80% when impregnated with flame retardant solution, and 60% when impregnated with resin glue.
[0044] Example 10
[0045] This embodiment provides a flame retardant reconstituted bamboo, and the preparation method is different from that of embodiment 1 only in that: The compression rate is 80% when impregnated with flame retardant solution, and 40% when impregnated with resin glue.
[0046] Comparative Example 1
[0047] This comparative example provides a flame retardant reconstituted bamboo, the preparation method of which is different from that of Example 1 only in that: Instead of mechanically squeezing and impregnating the flame retardant, the bamboo bundles with a moisture content of 10% are immersed in the flame retardant solution for 4 hours; instead of mechanically squeezing and impregnating the resin glue, the bamboo bundles impregnated with the flame retardant are immersed in the resin glue for 10 minutes.
[0048] Comparative Example 2
[0049] This comparative example provides a flame retardant reconstituted bamboo, the preparation method of which is different from that of Example 1 only in that: The concentration of the mixed flame retardant solution is 35%, and the flame retardant is not impregnated by mechanical extrusion. Instead, the bamboo bundles with a moisture content of 10% are immersed in the flame retardant solution for 4 hours; the resin glue is not impregnated by mechanical extrusion. Instead, the bamboo bundles impregnated with the flame retardant are immersed in the resin glue for 10 minutes.
[0050] Test Example 1
[0051] This test example tests the loss rate of flame retardant during the secondary impregnation process, and the steps are as follows: immerse the reconstructed bamboo unit of moso bamboo in a 30% concentration of diammonium hydrogen phosphate solution for 2 hours, take out and drain the excess liquid, and dry it to a moisture content of 10%. The reconstructed bamboo unit after flame retardant treatment is divided into two groups, one of which is immersed in water at normal pressure, and the other group is immersed in water by mechanical extrusion method (compression rate is 60%) to simulate the conventional dipping and mechanical extrusion dipping processes respectively. The flame retardant loss rate in the two groups of reconstructed bamboo units is calculated by weighing method, and the phosphorus content in the phenolic resin after impregnation is determined by organic element analyzer. The results are shown in Table 1.
[0052] Table 1 Flame retardant loss rate of reconstituted bamboo units impregnated at normal pressure and mechanical extrusion
[0053] As shown in Table 1, since the conventional impregnation method usually takes a long time, a large amount of flame retardant is lost in the process, resulting in a decrease in the content of flame retardant effective ingredients in the reconstructed bamboo, a decrease in flame retardant performance, and glue pollution. Compared with the conventional impregnation method, when the mechanical extrusion impregnation method is used for impregnation, the flame retardant reconstructed bamboo unit only needs to stay in the glue for a few seconds, reducing the flame retardant loss rate to 6.8%, and the phosphorus content of the solution after impregnation is significantly reduced, which shows that this method effectively solves the problem of flame retardant loss during the impregnation process, avoids glue pollution, ensures the reusability of the glue, and saves costs.
[0054] Test Example 2
[0055] This test example tests the flame retardant properties of the flame retardant reconstituted bamboo prepared in the above examples and comparative examples. The specific method is: referring to the ISO5660-1 standard, the pressed reconstituted bamboo is sawn into test pieces of a certain size, and the heat release performance is tested using a cone calorimeter. The flame retardant properties are tested from aspects such as the peak heat release rate and the total heat release (THR) and the flame retardant grade is evaluated. The test results are shown in Table 2.
[0056] Table 2 Flame retardant properties of flame retardant reconstructed bamboo
[0057] As shown in Table 2, as the number of compressions increases from 2 times (Example 1) to 4 times (Example 2), the amount of flame retardant added increases; the amount of flame retardant added by impregnating a 25% concentration flame retardant solution twice by mechanical extrusion is 22% (Example 1), which is basically the same as the amount of addition achieved by impregnating a 35% concentration flame retardant solution for 2 hours by conventional method (Comparative Example 2), indicating that the preparation method of the present invention can effectively improve the efficiency of flame retardant impregnation. At the same time, as the solid content of the resin increases, the amount of sizing increases, and the flame retardant performance gradually improves. When the compression rate increases, the amount of flame retardant added increases, and the flame retardant performance of the reconstructed bamboo gradually improves. Excessive compression rate (80%) causes serious damage to the reconstructed bamboo unit, and the water retention capacity deteriorates, resulting in a decrease in the amount of flame retardant added. However, at this time, the flame retardant is more evenly distributed in the reconstructed bamboo unit, and the flame retardant performance is optimal. Comparing Example 3 with Comparative Example 2, it can be seen that the flame retardant reconstructed bamboo prepared by mechanical extrusion has better flame retardant performance than the conventional method. All embodiments have reached B1 (C) level and above, which can meet the flame retardant grade requirements of most building constructions and greatly broaden the application scenarios of reconstructed bamboo.
[0058] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing flame retardant reconstituted bamboo, characterized in that: include: The reconstructed bamboo units are mechanically extruded in a flame retardant solution, impregnated with flame retardant during the process of releasing the mechanical pressure, and then mechanically extruded in a resin solution, so that the resin is absorbed into the cell cavity of the reconstructed bamboo units during the process of releasing the mechanical pressure, and then the assembly is hot-pressed to obtain the flame-retardant reconstructed bamboo.
2. The preparation method according to claim 1, characterized in that: The mechanical pressing is performed using a flat press or a roller press.
3. The preparation method according to claim 1, characterized in that: The compression rate of mechanically squeezed reconstructed bamboo units is 30%-80%.
4. The preparation method according to claim 1, characterized in that: After impregnation with the flame retardant, the reconstituted bamboo unit is dried to a moisture content of 8%-15%.
5. The preparation method according to claim 1, characterized in that: The reconstituted bamboo unit after adsorbing the resin is dried to a moisture content of 8%-15%.
6. The preparation method according to claim 1, characterized in that: The density of the flame retardant reconstituted bamboo is 0.80-1.30 g / cm 3 .
7. The preparation method according to claim 1, characterized in that: The flame retardant solution contains at least one of ammonium phosphate, ammonium sulfate, boron compounds and urea; the concentration of the flame retardant solution is 10%-50%.
8. The preparation method according to claim 1, characterized in that: The preparation method of the recombinant bamboo unit includes: sawing bamboo into bamboo tubes of a certain length, splitting into bamboo slices, and forming fiberized recombinant bamboo units through a decomposition machine, and drying to a moisture content of 8%-15%.
9. The preparation method according to claim 1, characterized in that: The bamboo species of the recombinant bamboo unit is a scattered bamboo species or a clumping bamboo species, preferably Phyllostachys pubescens, Phyllostachys cycads or Phyllostachys edulis.
10. The flame retardant reconstituted bamboo obtained by the preparation method according to any one of claims 1 to 9.