Composite nano aerogel insulation board and preparation method thereof

By sewing fabric layers on the outer nano-aerogel felt and combining them with silicone materials and reinforcement materials, the problem of insufficient structural strength of the kapok aerogel insulation board is solved, the tensile strength and insulation effect are improved, and high-temperature and high-pressure molding is achieved Low cost and environmentally friendly thermal insulation effect of the process.

CN118876512APending Publication Date: 2024-11-01JIANGSU SHENGWO ENERGY-SAVING NEW MATERIAL CO LTD

Patent Information

Application Number
CN202411019245.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing kapok aerogel insulation board has low compression strength and tensile strength, which can easily disperse protrusions and powder loss during transportation and installation, resulting in reduced insulation performance, and insufficient structural strength of the outer and bottom plates, which cannot meet the construction related aspects. standard.

Method used

Using composite nano-aerogel insulation board, the fabric layer is fabricated on the outer seam of nano-aerogel felt and combined with siliceous material and reinforcement material, connected through sewing thread, increasing the tensile strength and overall strength, and through high temperature and high pressure Preparation of molding process.

Benefits of technology

It effectively improves the tensile strength and bending ability of the plate body, enhances the overall strength, and ensures the insulation effect. At the same time, it is simple in process, low in cost, pollution-free, energy-saving and emission-reducing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118876512A_ABST
    Figure CN118876512A_ABST
Patent Text Reader

Abstract

The invention discloses a composite nano aerogel insulation board and a preparation method thereof, and relates to the technical field of building insulation boards, the inner layer of a board body comprises a nano aerogel felt, and the nano aerogel felt is wrapped and sewn by a cloth layer; the insulation board is prepared by laying a siliceous material, a reinforcing material and a nano aerogel felt wrapped with a cloth layer in a special mold in a layered manner according to requirements, and carrying out hot press molding. The nano aerogel felt is pretreated, dispersed protrusions and particle falling of the nano aerogel felt are avoided, the tensile strength and the bending resistance of the inner layer of the plate body are enhanced, meanwhile, the heat preservation effect is effectively guaranteed, and the reinforcing material is embedded into the inner layer of the plate body, so that the overall strength of the plate body is further improved. The invention also discloses a preparation method of the composite nano aerogel insulation board, which adopts a high-temperature hot press molding process, and has the advantages of simple flow, low cost, no pollution, energy conservation and emission reduction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of building insulation boards, in particular to a composite nano-aerogel insulation board and a preparation method thereof. Background Art

[0002] Insulation board is a rigid foam plastic board made of polystyrene resin as raw material, combined with other raw and auxiliary materials and polymers, which is made by heating and mixing, injecting a catalyst, and then extruding and pressing into shape. The insulation board has moisture-proof and waterproof properties, which can reduce the thickness of the building's external protective structure, thereby increasing the indoor usable area and can be used for building insulation. Types include EPS insulation board, STP insulation board, etc. Nano aerogel insulation board is a nano rigid insulation board that can be used in construction, warehouses, equipment and other fields to meet the insulation and heat insulation requirements of different customers for insulation layer thickness, heat resistance and strength to the greatest extent. Nano aerogel is the substance with the lowest thermal conductivity among solids known to date. Nano aerogel insulation board has become the best choice for users seeking better insulation effects due to its extremely low thermal conductivity, energy saving and environmental protection, ease of use and excellent hydrophobic effect, especially in the field of external insulation in ultra-low energy consumption buildings.

[0003] Patent publication number CN109763576A discloses a kapok aerogel thermal insulation board, comprising: a faceplate, a baseplate, and an insulation core plate. The faceplate and baseplate are fixedly attached to the upper and lower surfaces of the insulation core plate, respectively, and the faceplate and baseplate are made of an inorganic gelling material. The insulation core plate is made of kapok aerogel as the main material, mixed with kapok flame-retardant fibers and inorganic gelling materials, stirred, foamed, and wrapped. The kapok aerogel is SiO2 aerogel prepared using a cracking method using kapok as the raw material. Although this technical solution utilizes the ultra-light density and ultra-low thermal conductivity of kapok aerogel and the high strength and flame retardant properties of inorganic gelling materials, it is more environmentally friendly than conventional silica nano-aerogel insulation products, has low cost, simple production process, low density, and better thermal insulation effect, but it still has the following problems:

[0004] (1) Since kapok aerogel has a layered loose structure, its compressive strength and tensile strength are low, especially the tensile strength perpendicular to the surface is even smaller. In addition, it is easy to bulge and fall off during transportation and installation, which will lead to a decrease in the thermal insulation performance of the overall insulation board.

[0005] (2) Conventional outer panels and base panels are made of only siliceous materials and are not reinforced with any reinforcing materials, resulting in low structural strength of the overall insulation board, which cannot meet the strength requirements of the relevant building standards for exterior wall insulation materials. Summary of the Invention

[0006] In view of the shortcomings of the existing technology, the present invention provides a composite nano-aerogel insulation board and a preparation method thereof, which solves the problem of affecting the overall structural strength of the board and the thermal insulation effect of the insulation board.

[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions: a composite nano-aerogel insulation board, comprising a board body, the board body comprising a nano-aerogel felt, a cloth layer sewn to the outside of the nano-aerogel felt, the nano-aerogel felt and the cloth layer being sewn together by sewing thread, the top and bottom of the cloth layer being provided with siliceous material, and the two sides of the siliceous materials being opposite to each other being provided with reinforcement material, and the two sides of the reinforcement materials being opposite to each other being provided with siliceous material;

[0008] The fabric layer is any one of canvas and aluminum foil cloth, and the sewing threads are arranged in any one of cross knitting, horizontal and vertical knitting or equidistant knitting.

[0009] Preferably, the raw material of the siliceous material is composed of a combination of siliceous gel material and polystyrene particles.

[0010] Preferably, the reinforcement material is any one of alkali-resistant mesh cloth and steel wire mesh, the mesh aperture is 12-100 mm, and the density of the polystyrene particles is 3-5 mg / cm 3 .

[0011] Preferably, the mass ratio of the silica gel material to the polystyrene particles is 1:2-1:5.

[0012] Preferably, the preparation method of the composite nano-aerogel insulation board specifically includes the following steps:

[0013] S1. Pretreatment of nano aerogel felt: Cut the nano aerogel felt to size, then wrap the fabric layer on the surface of the nano aerogel felt, and then sew the nano aerogel felt and the fabric layer together with sewing thread. The sewing method adopts the longitudinal and transverse directions to make it more tight, and apply adhesive on both sides;

[0014] S2. Preparation of siliceous material: Add silica gel material and polystyrene particles into a dispersion kettle, use purified water as a medium, fully disperse at 40°C, 1000 r / min for 30 minutes to obtain a dispersion liquid, then heat and dry at a temperature of 170-200°C to obtain a mixed powder, then add a foaming agent, an inorganic adhesive, a high-hardness filler and a curing agent, fully mix at 1000 r / min for 30-60 minutes, and then introduce steam for heating and fully foaming. The foamed bulk density is 10.5-20 kg / m3 to obtain a siliceous material raw material;

[0015] S3. Preparation of the board: The siliceous material, reinforcement material, siliceous material, nano-aerogel felt wrapped with a cloth layer, siliceous material, reinforcement material and siliceous material obtained in S2 are layered in a special mold in sequence. After laying, the whole is subjected to high temperature and high pressure treatment, and pressed downward in the mold with the temperature controlled at 80-105°, the time controlled at 1-3 hours, and the pressure controlled at 0.4-5MPa to obtain the board.

[0016] Preferably, in S2, the siliceous material is composed of the following components: 10-20 parts of siliceous gel material, 10-20 parts of polystyrene particles, 30-50 parts of purified water, 5-15 parts of foaming agent, 10-20 parts of inorganic adhesive, 12-22 parts of high hardness filler and 10-16 parts of curing agent.

[0017] Beneficial effects

[0018] The present invention provides a composite nano-aerogel insulation board and a preparation method thereof. Compared with the prior art, it has the following advantages:

[0019] (1) The present invention discloses a composite nano-aerogel insulation board and a preparation method thereof, wherein the nano-aerogel felt is pre-treated, wrapped with a cloth layer, and sewn into shape, thereby avoiding the scattered protrusions and particle shedding of the nano-aerogel felt, enhancing the tensile strength and bending resistance of the inner layer of the board body, and effectively ensuring the thermal insulation effect.

[0020] (2) The present invention discloses a composite nano-aerogel insulation board and a preparation method thereof, wherein a reinforcing material is embedded in the inner layer of the board body. The reinforcing material can be an alkali-resistant mesh cloth or a steel wire mesh, so that the overall strength of the board body is further improved.

[0021] (3) The present invention discloses a composite nano-aerogel insulation board and a preparation method thereof, which adopts a high-temperature hot pressing molding process, has a simple process, low cost, is pollution-free, and saves energy and reduces emissions. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A perspective view of the structure of the present invention;

[0023] Figure 2 is a cross-sectional view of the structure of the present invention;

[0024] Figure 3 This is a diagram of different sewing methods for the sewing thread of the present invention.

[0025] In the figure: 1-plate, 11-nano aerogel felt, 12-cloth layer, 13-sewing thread, 14-silica material, 15-reinforcement material. DETAILED DESCRIPTION

[0026] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0027] See also Figure 1-3 The present invention provides two technical solutions: a composite nano-aerogel insulation board, comprising a board body 1, the board body 1 comprising a nano-aerogel felt 11, a cloth layer 12 sewn to the outside of the nano-aerogel felt 11, the nano-aerogel felt 11 and the cloth layer 12 being sewn together by sewing thread 13, a siliceous material 14 being provided on the top and bottom of the cloth layer 12, and a reinforcing material 15 being provided on the opposite sides of the two siliceous materials 14, and a siliceous material 14 being provided on the opposite sides of the two reinforcing materials 15;

[0028] The fabric layer 12 is any one of canvas and aluminum foil, and the sewing threads 13 are arranged in any one of cross knitting, horizontal and vertical knitting or equidistant knitting.

[0029] In the present invention, the raw material of the siliceous material 14 is composed of a combination of siliceous gel material and polystyrene particles.

[0030] In the present invention, the reinforcing material 15 is any one of an alkali-resistant mesh cloth and a steel mesh, the mesh aperture is 12-100 mm, and the density of the polystyrene particles is 3-5 mg / cm 3 .

[0031] In the present invention, the mass ratio of the silica gel material to the polystyrene particles is 1:2-1:5.

[0032] The present invention also discloses a method for preparing a composite nano-aerogel insulation board, which specifically includes the following embodiments:

[0033] Example 1

[0034] S1. Pretreatment of the nano aerogel felt 11: cutting the nano aerogel felt 11 to size, then wrapping the fabric layer 12 on the surface of the nano aerogel felt 11, and then sewing the nano aerogel felt 11 and the fabric layer 12 together with sewing thread 13. The sewing method adopts the longitudinal and transverse directions to make it more tight, and applying adhesive on both sides;

[0035] S2. Preparation of siliceous material 14: 15 parts of silica gel material and 15 parts of polystyrene particles were added to a dispersion kettle, and the mixture was fully dispersed at 40° C. and 1000 rpm for 30 minutes using 40 parts of purified water as a medium to obtain a dispersion liquid. The mixture was then heated and dried at 185° C. to obtain a mixed powder. 10 parts of a foaming agent, 15 parts of an inorganic adhesive, 17 parts of a high-hardness filler, and 13 parts of a curing agent were then added, and the mixture was fully mixed at 1000 rpm for 45 minutes. Steam was then introduced for heating to fully foam the mixture, and the foamed bulk density was 15 kg / m 3 to obtain a raw material of siliceous material 14.

[0036] S3. Preparation of the plate body 1: The siliceous material 14, the reinforcing material 15, the siliceous material 14, the nano-aerogel felt 11 wrapped with the cloth layer 12, the siliceous material 14, the reinforcing material 15 and the siliceous material 14 obtained in S2 are layered in sequence in a special mold. After laying, the whole is subjected to high temperature and high pressure treatment, and pressed downward in the mold with the temperature controlled at 95° for 2 hours and the pressure controlled at 5 MPa to obtain the plate body 1.

[0037] Example 2

[0038] S1. Pretreatment of the nano aerogel felt 11: cutting the nano aerogel felt 11 to size, then wrapping the fabric layer 12 on the surface of the nano aerogel felt 11, and then sewing the nano aerogel felt 11 and the fabric layer 12 together with sewing thread 13. The sewing method adopts the longitudinal and transverse directions to make it more tight, and applying adhesive on both sides;

[0039] S2. Preparation of siliceous material 14: 20 parts of silica gel material and 20 parts of polystyrene particles were added to a dispersion kettle, and fully dispersed at 40°C and 1000 rpm for 30 minutes using 50 parts of purified water as a medium to obtain a dispersion liquid. The mixture was then heated and dried at 200°C to obtain a mixed powder. 5-15 parts of a foaming agent, 20 parts of an inorganic adhesive, 22 parts of a high-hardness filler, and 16 parts of a curing agent were then added, and the mixture was fully mixed at 1000 rpm for 60 minutes. Steam was then introduced for heating to fully foam the mixture, and the foamed bulk density was 20 kg / m3 to obtain a raw material of siliceous material 14.

[0040] S3. Preparation of the plate body 1: The siliceous material 14, the reinforcing material 15, the siliceous material 14, the nano-aerogel felt 11 wrapped with the cloth layer 12, the siliceous material 14, the reinforcing material 15 and the siliceous material 14 obtained in S2 are layered in sequence in a special mold. After laying, the whole is subjected to high temperature and high pressure treatment, and pressed downward in the mold with the temperature controlled at 105°, the time for 3 hours, and the pressure controlled at 3 MPa to obtain the plate body 1.

[0041] Example 3

[0042] S1. Pretreatment of the nano aerogel felt 11: cutting the nano aerogel felt 11 to size, then wrapping the fabric layer 12 on the surface of the nano aerogel felt 11, and then sewing the nano aerogel felt 11 and the fabric layer 12 together with sewing thread 13. The sewing method adopts the longitudinal and transverse directions to make it more tight, and applying adhesive on both sides;

[0043] S2. Preparation of siliceous material 14: 10 parts of silica gel material and 10 parts of polystyrene particles were added to a dispersion kettle, and the mixture was fully dispersed at 40° C. and 1000 rpm for 30 minutes using 30 parts of purified water as a medium to obtain a dispersion liquid. The mixture was then heated and dried at 170° C. to obtain a mixed powder. 5 parts of a foaming agent, 10 parts of an inorganic adhesive, 12 parts of a high-hardness filler, and 10 parts of a curing agent were then added, and the mixture was fully mixed at 1000 rpm for 30 minutes. Steam was then introduced for heating to fully foam the mixture, and the foamed bulk density was 10.5 kg / m 3 to obtain a raw material of siliceous material 14.

[0044] S3. Preparation of the plate body 1: The siliceous material 14, the reinforcing material 15, the siliceous material 14, the nano-aerogel felt 11 wrapped with the cloth layer 12, the siliceous material 14, the reinforcing material 15 and the siliceous material 14 obtained in S2 are layered in sequence in a special mold. After laying, the whole is subjected to high temperature and high pressure treatment, and pressed downward in the mold with the temperature controlled at 85°, the time for 1 hour, and the pressure controlled at 4 MPa to obtain the plate body 1.

[0045] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.

[0046] Effect embodiment

[0047] A thermal insulation board manufacturer tested the thermal insulation boards produced in Examples 1, 2, and 3, respectively, as well as commonly used thermal insulation boards on the market, for compressive strength according to GB / T5486-2008, "Test Methods for Inorganic Rigid Thermal Insulation Products," for tensile strength according to GB / T29906-2013, "Molded Polystyrene Board Thin-Plaster Exterior Wall Insulation System Materials," for thermal conductivity according to GB / T10294-2008, "Thermal Insulation Materials - Determination of Steady-State Thermal Resistance and Related Properties - Guarded Hot Plate Method," for flexural deformation according to GB / T10801.1, "Molded Polystyrene Foam for Thermal Insulation," and for combustion performance according to GB8624-2012, "Classification of Combustion Behavior of Building Materials and Products." Furthermore, the manufacturer tested the boards for breaking bending load and wear resistance. During the testing process, statistical data was collected and statistical tables and graphs were prepared.

[0048]

[0049] As can be seen from the table above, the nano-aerogel felt is wrapped in canvas or aluminum foil, sewn together in multiple strips horizontally and vertically. When the insulation board comes into contact with water, the nano-aerogel felt will not disperse or bulge. The canvas shapes the nano-aerogel felt, increasing its strength without affecting the insulation effect of the insulation board. Silicon material is wrapped on both sides after foaming, reinforced with material, and then placed in layers in a special mold for hot pressing. This can effectively improve the overall thermal insulation performance of the insulation board and enhance its overall strength.

[0050] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions, and variations may be made to these embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the appended claims and their equivalents.

Claims

1. A composite nano-aerogel thermal insulation board, comprising a board body (1), characterized in that: The plate body (1) comprises a nano aerogel felt (11), a cloth layer (12) is sewn on the outside of the nano aerogel felt (11), the nano aerogel felt (11) and the cloth layer (12) are sewn together by sewing thread (13), a siliceous material (14) is provided on the top and bottom of the cloth layer (12), and a reinforcing material (15) is provided on the opposite sides of the two siliceous materials (14), and a siliceous material (14) is provided on the opposite sides of the two reinforcing materials (15); The fabric layer (12) is any one of canvas and aluminum foil, and the sewing threads (13) are arranged in any one of cross knitting, horizontal and vertical knitting or equidistant knitting.

2. The composite nano-aerogel insulation board according to claim 1, characterized in that: The raw material of the siliceous material (14) is a combination of siliceous gel material and polyphenylene particles.

3. The composite nano-aerogel insulation board according to claim 1, characterized in that: The reinforcing material (15) is any one of an alkali-resistant mesh cloth and a steel wire mesh, the mesh aperture is 12-100 mm, and the density of the polystyrene particles is 3-5 mg / cm 3 .

4. The composite nano-aerogel thermal insulation board according to claim 2, characterized in that: The mass ratio of the silica gel material to the polyphenylene particles is 1:2-1:

5.

5. A composite nano-aerogel insulation board according to any one of claims 1 to 4, wherein the preparation method thereof specifically comprises the following steps: S1. Pretreatment of the nano aerogel felt (11): cutting the nano aerogel felt (11) to a certain size, then wrapping the fabric layer (12) on the surface of the nano aerogel felt (11), and then sewing the nano aerogel felt (11) and the fabric layer (12) together using sewing threads (13), wherein the sewing method uses longitudinal and transverse alignment to make it more secure, and applying adhesive on both sides; S2, preparation of siliceous material (14): add siliceous gel material and polystyrene particles into a dispersion kettle, use purified water as a medium, fully disperse for 30 minutes at 40°C and 1000r / min to obtain a dispersion liquid, then heat and dry at a temperature of 170-200°C to obtain a mixed powder, then add a foaming agent, an inorganic adhesive, a high-hardness filler and a curing agent, fully mix for 30-60 minutes at 1000r / min, then pass steam to heat, fully foam, and the foamed bulk density is 10.5-20kg / m3 to obtain a siliceous material (14) raw material; S3, preparation of the plate body (1): the siliceous material (14), reinforcing material (15), siliceous material (14), nano-aerogel felt (11) wrapped with a cloth layer (12), siliceous material (14), reinforcing material (15) and siliceous material (14) obtained in S2 are sequentially layered in a special mold, and after being laid, the whole is subjected to high temperature and high pressure treatment, and pressed downward in the mold with the temperature controlled at 80-105°, the time controlled at 1-3 hours, and the pressure controlled at 0.4-5MPa, to obtain the plate body (1).

6. The method for preparing a composite nano-aerogel insulation board according to claim 5, characterized in that: In the S2, the siliceous material (14) is composed of the following components: 10-20 parts of siliceous gel material, 10-20 parts of polyphenyl particles, 30-50 parts of purified water, 5-15 parts of foaming agent, 10-20 parts of inorganic adhesive, 12-22 parts of high hardness filler and 10-16 parts of curing agent.

Citation Information

Patent Citations

  • Bombax ceiba aerogel thermal insulation board

    CN109763576A

  • Thermal insulation material and thermal insulation board

    CN110950617A

  • Composite insulation board as well as preparation method and application thereof

    CN112874046A

  • Fireproof insulation board with built-in efficient insulation layer, preparation method and building energy-saving structure

    CN116427565A

  • Aerogel energy-saving thermal insulation felt

    CN204284800U

Cited By

  • Inorganic composite insulation board with thermal insulation function and preparation method thereof

    CN120716252A