Preparation method of moisture-absorbing and quick-drying non-woven fabric
Through the preparation method of non-woven fabrics with two-sided structures, combined with hydrospuncture processing and hot air bonding technology, the problem of insufficient moisture absorption and quick drying function of traditional non-woven fabrics on the waist of diapers is solved, and the effect of efficient moisture absorption and rapid drying is achieved, which improves the effect of improved Comfort for sanitary products.
Patent Information
- Application Number
- CN202411157956.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-22
AI Technical Summary
Traditional non-woven fabrics lack moisture absorption and quick drying when applied to the waistline of diapers, resulting in low comfort.
The preparation method of non-woven fabrics with two-sided structures is adopted, long fibers are used on the immersion surface and short fibers are used on the permeable surface. The composite non-woven fabric is formed by hydrospinning processing. The permeable surface fibers are ≥5% tangled with the immersed surface, and the immersed surface fibers are <3% , and prepared by twin screw extruder and hot air bonding technology, the temperature and stretch ratio are controlled to improve hygroscopicity and hydrophilicity.
The preparation of moisture-absorbing and fast-drying non-woven fabric is realized, wicking height ≥80mm, drying rate ≥0.2g/h, drip diffusion time ≤6s, water absorption rate ≥300%, and one-way transmission index ≥100, which improves disposable sanitary products Comfortable waist.
Abstract
Description
Technical Field
[0001] The invention relates to the field of sanitary products, and in particular to a method for preparing a moisture-absorbing and quick-drying non-woven fabric. Background Art
[0002] With the development of science and technology, people's living standards are constantly improving. As a disposable product, non-woven fabrics occupy an important position in people's lives, especially in the waistline of pants diapers, menstrual pants, and disposable underwear.
[0003] Traditional non-woven fabrics are generally made of PP fibers, which have a hard feel, rough fibers, and are relatively uncomfortable to wear. In order to improve the performance of non-woven fabrics, Chinese Patent Publication No. CN117103792A discloses a preparation process for a five-layer heterogeneous ultra-soft non-woven fabric, the preparation process comprising: preparing a spunbond layer: mixing the raw materials of the spunbond layer according to a ratio, and then subjecting them to screw extrusion melting, metered spinning, cold air drawing, and web laying to obtain a spunbond layer; meltblown layer: mixing the raw materials of the meltblown layer according to a ratio, and subjecting them to screw extrusion melting, metered spinning, hot air drawing, and web laying to obtain a meltblown layer; a five-layer fiber web structure of two spunbond layers, two meltblown layers, and one spunbond layer from the outside to the inside, hot rolling the five-layer structure, and then drying it to obtain a SSMMS five-layer heterogeneous ultra-soft non-woven fabric. The five-layer non-woven fabric has good mechanical properties and strength and is ultra-flexible, and can be used for the inner / outer waist of diapers. However, the non-woven fabric of this structure does not have the characteristics of moisture absorption and quick drying. When used in the waist of diapers, there is a lot of room for improvement in the comfort of use. Summary of the invention
[0004] Therefore, in view of the above problems, the present invention provides a method for preparing a moisture-absorbing and quick-drying non-woven fabric, which solves the defect that the non-woven fabric obtained by the preparation method of the prior art does not have the moisture-absorbing and quick-drying function.
[0005] To achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a method for preparing a moisture-absorbing and quick-drying non-woven fabric, comprising the following preparation steps: (1) preparation of raw materials, including a water-immersed surface raw material and a permeable surface raw material, wherein the water-immersed surface raw material is long fibers and the permeable surface raw material is short fibers; (2) preparation of the water-immersed surface non-woven fabric: laying the long fibers on a web to process them into a water-immersed surface non-woven fabric; (3) preparation of the permeable surface non-woven fabric: laying the short fibers on a web to obtain a permeable surface non-woven fabric with a surface densely covered with mesh holes; (4) preparation of the non-woven fabric: hydroentanglement of the water-immersed surface non-woven fabric obtained in step (2) and the permeable surface non-woven fabric obtained in step (3) to form a moisture-absorbing and quick-drying non-woven fabric, wherein after the hydroentanglement, more than 5% of the fibers on the permeable surface are entangled with the water-immersed surface, and less than 3% of the fibers on the water-immersed surface are entangled with the permeable surface.
[0006] Further: the raw material of the immersion surface is polypropylene or two-component PE / PP and hydrophilic masterbatch, and the raw material of the permeable surface is bamboo fiber or kapok fiber or pure cotton fiber or viscose fiber or lyocell fiber or modal fiber.
[0007] Furthermore: the fineness of the short fibers is 1.0-2.2 dtex.
[0008] Further: the weight of the permeable surface material is 10-30gsm, and the weight of the water-immersed surface material is 5-20gsm.
[0009] Further: the mesh size of the permeable surface non-woven fabric is 10-40 meshes.
[0010] Furthermore: the surface of the long fiber has a non-smooth and non-circular structure, such as a groove or a hollow or special-shaped cross-section or a natural curved structure.
[0011] Furthermore, the preparation method of the water-immersed nonwoven fabric is specifically as follows: (1) using PP masterbatch and PE masterbatch as raw materials, drying the raw materials so that the moisture content of the PP masterbatch and the PE masterbatch is less than 0.1%;
[0012] (2) feeding the raw materials into a twin-screw extruder for melt extrusion and composite spinning, and in the composite spinning process, the PP melt and the PE melt are respectively passed through the PP pipe and the PE pipe for heat preservation and then merged at the spinneret hole, the temperature of the PP pipe is maintained at 240-250° C., the temperature of the PE pipe is maintained at 260-275° C., and the temperature of the spinning box is controlled at 265-275° C.;
[0013] (3) cooling, forming, oiling, winding, drawing, curling, shaping, and slitting to obtain long fibers, wherein the melt index of the PP masterbatch is 20-30 g / 10 min, and the melt index of the PE masterbatch is 15-25 g / 10 min;
[0014] (4) hot-air bonding the long fibers to form a water-immersed nonwoven fabric;
[0015] (5) Punching process.
[0016] Furthermore: the volume ratio of the PP masterbatch to the PE masterbatch is 1:1-1.2.
[0017] Further: the stretching treatment adopts two-stage stretching, the first stage stretching multiple is 3-4, and the second stage stretching multiple is 1.02-1.1.
[0018] Further: during cooling and forming, side blowing with a temperature of 15-22°C and a wind speed of 0.5-0.9m / s is adopted.
[0019] By adopting the above-mentioned technical scheme, the beneficial effects of the present invention are as follows: 1. The moisture-absorbing and quick-drying non-woven fabric of the present invention has a two-sided structure, one side is a water-immersed side, and the other side is a permeable side. The raw materials used for the two-sided structural layers are different. The permeable side is made of long fibers, and the water-immersed side is made of short fibers. The composite non-woven fabric is then compounded by a spunlace process. The processed permeable side of the composite non-woven fabric has better hygroscopicity and hydrophilicity than the water-immersed side. When applied to the waist non-woven fabric of disposable sanitary products, it can play a role of moisture absorption and quick drying.
[0020] 2. The moisture-absorbing and quick-drying non-woven fabric obtained by the preparation method of the present invention has a wicking height of ≥80 mm, a drying rate of ≥0.2 g / h, no mirror reflection when absorbing liquid, a drip diffusion time of ≤6 s, a water absorption rate of ≥300%, a water absorption rate of the immersed surface of ≥30% / s, a water absorption rate of the permeable surface of ≥30% / s, and a one-way transfer index of ≥100, referring to standards GB / T 21665.1 and GB / T21665.2.
[0021] 3. Furthermore, in the preparation process of the non-woven fabric with the immersed surface, PE and PP have similar fluidity, which makes it difficult to separate during compounding. The melting point of PE is relatively low, about 130°C, and the melting point of PP is 170°C. When heated to 130°C, the skin layer PE is melted and bonded to each other, and the PP core layer remains in a fiber state, providing physical support. PP is bulky, PE is soft and tough, and the overall feel is good. The PP pipe and PE pipe are kept in a relatively reasonable temperature range, so that the skin layer and the core layer are more evenly distributed, and it is not easy to break during spinning and stretching.
[0022] 4. The stretching treatment adopts two-stage stretching. The first stage stretching is mainly to thin the inside of the fiber, eliminate the internal stress between macromolecules under the action of external force, reduce the shrinkage rate of the fiber, and improve the shrinkage strength. The second stage stretching is to further orient and crystallize the macromolecules and perform tense heat setting to reduce the thermal shrinkage of the fiber in the production of nonwoven fabrics. By controlling the ratio of the two-stage stretching, the obtained two-component fiber is made bulky and soft. DETAILED DESCRIPTION
[0023] The embodiments of the present invention are:
[0024] A method for preparing a moisture-absorbing quick-drying nonwoven fabric comprises the following preparation steps: (1) preparing raw materials, including a water-immersed surface raw material and a permeable surface raw material, wherein the water-immersed surface raw material is long fibers and the permeable surface raw material is short fibers; (2) preparing the water-immersed surface nonwoven fabric: laying the long fibers on a web to form a water-immersed surface nonwoven fabric; (3) preparing the permeable surface nonwoven fabric: laying the short fibers on a web to obtain a permeable surface nonwoven fabric with a surface densely covered with mesh holes; (4) preparing the nonwoven fabric: hydroentanglement-processing the water-immersed surface nonwoven fabric obtained in step (2) and the permeable surface nonwoven fabric obtained in step (3) to form a moisture-absorbing quick-drying nonwoven fabric, wherein after the hydroentanglement processing, more than 5% of the fibers on the permeable surface are entangled with the water-immersed surface, and less than 3% of the fibers on the water-immersed surface are entangled with the permeable surface.
[0025] The preparation method of the water-immersed nonwoven fabric is as follows: a. Using PP masterbatch and PE masterbatch as raw materials, drying the raw materials to make the moisture content of the PP masterbatch and the PE masterbatch 0.05%;
[0026] b. The raw materials are fed into a twin-screw extruder for melt extrusion and composite spinning. During the composite spinning process, the PP melt and the PE melt are respectively heat-insulated through the PP pipe and the PE pipe and then merged at the spinneret hole. The temperature of the PP pipe is maintained at 240° C., the temperature of the PE pipe is maintained at 260° C., and the temperature of the spinning box is controlled at 265° C.;
[0027] c. Cooling, forming, oiling, winding, drawing, curling, shaping, and slitting to obtain short fibers, wherein the melt index of the PP masterbatch is 20g / 10min, and the melt index of the PE masterbatch is 15g / 10min; the stretching treatment adopts two-stage stretching, the first-stage stretching multiple is 3, and the second-stage stretching multiple is 1.1; during cooling and forming, a side blowing air with a temperature of 22°C and a wind speed of 0.5m / s is adopted;
[0028] d. hot-air bonding the long fibers to form a water-immersed nonwoven fabric: the long fibers are loosened, mixed, combed, and hot-air bonded;
[0029] e. Punching process.
[0030] The obtained short fiber fineness is 1.0 dtex; the gram weight of the permeable surface material is 10 gsm, and the mesh size of the permeable surface non-woven fabric is 40 meshes; the volume ratio of the PP masterbatch to the PE masterbatch is 1:1.1.
[0031] In this embodiment, the fiber used for the permeable surface is viscose fiber, which has been processed to have a hollow structure on the surface, so that the liquid can be discharged quickly.
[0032] In addition, a small amount of hydrophilic masterbatch can be added to the long fibers used for the water-immersed surface nonwoven fabric of the present invention during the preparation process. Specifically, a hydrophilic oil agent can be added during the oiling process to increase the hydrophilicity of the water-immersed surface nonwoven fabric.
[0033] With reference to standards GB / T 21665.1 and GB / T 21665.2, the moisture-absorbing and quick-drying nonwoven fabric obtained by the preparation method of the present invention has a wicking height of ≥80 mm, a drying rate of ≥0.2 g / h, no mirror reflection when absorbing liquid, a drip diffusion time of ≤6 s, a water absorption rate of ≥300%, a water absorption rate of ≥30% / s on the immersion surface, and a water absorption rate of ≥0.2 g / h on the penetration surface.
[0034] ≥30% / s, one-way transfer index ≥100.
[0035] Although the present invention has been specifically shown and described in conjunction with the preferred embodiments, it should be understood by those skilled in the art that various changes may be made to the present invention in form and details without departing from the spirit and scope of the present invention as defined by the appended claims, all of which are within the scope of protection of the present invention.
Claims
1. A method for preparing a moisture-absorbing quick-drying nonwoven fabric, characterized in that: The method comprises the following preparation steps: (1) preparing raw materials, including raw materials for a water-immersed surface and raw materials for a permeable surface, wherein the raw materials for the water-immersed surface are long fibers and the raw materials for the permeable surface are short fibers; (2) preparing a non-woven fabric for the water-immersed surface: laying the long fibers on a web to form a water-immersed surface non-woven fabric; (3) preparing a non-woven fabric for the permeable surface: laying the short fibers on a web to form a permeable surface non-woven fabric with a surface densely covered with mesh holes; (4) preparing a non-woven fabric: hydroentangling the water-immersed surface non-woven fabric obtained in step (2) and the permeable surface non-woven fabric obtained in step (3) to form a moisture-absorbing and quick-drying non-woven fabric, wherein after the hydroentangling process, more than 5% of the fibers on the permeable surface are entangled with the water-immersed surface, and less than 3% of the fibers on the water-immersed surface are entangled with the permeable surface.
2. The method for preparing a moisture-absorbing and quick-drying nonwoven fabric according to claim 1, characterized in that: The raw material of the immersion surface is polypropylene or two-component PE / PP and hydrophilic masterbatch, and the raw material of the permeable surface is bamboo fiber or kapok fiber or pure cotton fiber or viscose fiber or lyocell fiber or modal fiber.
3. The method for preparing a moisture-absorbing and quick-drying nonwoven fabric according to claim 1, characterized in that: The fineness of the short fibers is 1.0-2.2 dtex.
4. The method for preparing a moisture-absorbing and quick-drying nonwoven fabric according to claim 1, characterized in that: The weight of the permeable surface material is 10-30gsm, and the weight of the submerged surface material is 5-20gsm.
5. The method for preparing a moisture-absorbing and quick-drying nonwoven fabric according to claim 1, characterized in that: The mesh size of the permeable non-woven fabric is 10-40 mesh.
6. The method for preparing a moisture-absorbing and quick-drying nonwoven fabric according to claim 2, characterized in that: The long fiber surface has a non-smooth and non-circular structure, such as a groove or a hollow or special-shaped cross-section or a natural curved structure.
7. The method for preparing a moisture-absorbing and quick-drying nonwoven fabric according to claim 1, characterized in that: The preparation method of the water-immersed nonwoven fabric is specifically as follows: (1) using PP masterbatch and PE masterbatch as raw materials, drying the raw materials so that the moisture content of the PP masterbatch and the PE masterbatch is less than 0.1%; (2) feeding the raw materials into a twin-screw extruder for melt extrusion and composite spinning, and in the composite spinning process, the PP melt and the PE melt are respectively passed through the PP pipe and the PE pipe for heat preservation and then merged at the spinneret hole, the temperature of the PP pipe is maintained at 240-250° C., the temperature of the PE pipe is maintained at 260-275° C., and the temperature of the spinning box is controlled at 265-275° C.; (3) cooling, forming, oiling, winding, drawing, curling, shaping, and slitting to obtain long fibers, wherein the melt index of the PP masterbatch is 20-30 g / 10 min, and the melt index of the PE masterbatch is 15-25 g / 10 min; (4) hot-air bonding the long fibers to form a water-immersed nonwoven fabric; (5) Punching process.
8. The method for preparing a moisture-absorbing and quick-drying nonwoven fabric according to claim 7, characterized in that: The volume ratio of the PP masterbatch to the PE masterbatch is 1:1-1.
2.
9. The method for preparing a moisture-absorbing and quick-drying nonwoven fabric according to claim 7, characterized in that: The stretching treatment adopts two-stage stretching, the first stage stretching ratio is 3-4, and the second stage stretching ratio is 1.02-1.
1.
10. The method for preparing a moisture-absorbing and quick-drying nonwoven fabric according to claim 7, characterized in that: During cooling and forming, side blowing air with a temperature of 15-22°C and a wind speed of 0.5-0.9m / s is used.
Citation Information
Patent Citations
Air filter cloth material
CN102698508A
Liquid-retaining sheet and face mask
CN104487629A
Lysimachia christinae Hance fiber antibacterial textile fabric and preparation method thereof
CN113089316A
Preparation process of golden flower honey mask cloth
CN115198443A
Polyamide and bioresourced reinforcement compositions having improved mechanical properties
FR2938847A1