Biaxially-oriented polypropylene (BOPP) double-sided heat-sealing film and preparation method thereof

By using modified fillers in the outer layer material of the BOPP double-sided heat seal film, combining silicon micropowder and graphene, the problem of insufficient dust resistance in the prior art is solved, and the dust resistance and wear resistance of the film is significantly improved , suitable for packaging materials with high temperature and microwave permeability requirements.

CN118876544AActive Publication Date: 2024-11-01GUANGDONG WEIFU PACKAGING MATERIAL
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410961589.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-01
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

The existing BOPP double-sided heat seal film has poor dust resistance, is easy to absorb dust, and is difficult to meet the requirements of high temperature and microwave permeability.

Method used

Add filler composed of silicon micropowder and graphene to the outer layer material of the BOPP double-sided heat seal film, and modify the modified filler to improve dust resistance. .

Benefits of technology

It significantly improves the dust resistance of BOPP double-sided heat seal film, reduces the amount of dust adsorption, and enhances the wear resistance and durability of packaging materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of BOPP (Biaxially-oriented Polypropylene) films, and particularly discloses a BOPP double-sided heat-sealing film and a preparation method thereof. The BOPP double-sided heat-sealing film comprises a core layer and an outer layer, and the core layer is made of homo-polypropylene resin; the outer layer is made of a polypropylene composition; the polypropylene composition comprises the following components: 80 to 120 parts of homo-polypropylene resin; 30 to 50 parts of filler; 1-3 parts of a lubricant; 0.5 to 2 parts of an antioxidant; the filler is composed of silica powder and graphene. Researches show that the filler composed of the silica powder and the graphene is added into the outer layer material of the BOPP double-sided heat-sealing film, so that the dustproof performance of the BOPP double-sided heat-sealing film can be remarkably improved; the important application value is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of BOPP film preparation, and in particular to a BOPP double-sided heat-sealed film and a preparation method thereof. Background Art

[0002] Since the 1990s, the rapid development of microwave heating technology has put forward new requirements for the packaging of microwave food and a class of commodities that need to be sterilized by microwaves, that is, the packaging materials must not only have excellent barrier properties, but also have characteristics such as high temperature resistance and good microwave permeability. Therefore, in recent years, new high-barrier packaging materials have been a research and development direction for many industrially developed countries in the world. This type of material has the advantages of good microwave permeability, high temperature resistance, transparency, and little influence by ambient temperature and humidity. It can be widely used in the packaging of a class of commodities such as food, medicine, cosmetics, and medical devices that have high requirements for packaging safety and sanitation performance and long shelf life. It is particularly suitable as a packaging material for a class of commodities that use microwave heating technology. For example, Chinese invention patent 201910319194.4 discloses a BOPP double-sided heat-sealing film and a preparation method thereof; the BOPP double-sided heat-sealing film includes a core layer (1) and an outer layer (3), and a sub-surface layer (2) is arranged between the core layer and the outer layer; wherein the material of the sub-surface layer is a polypropylene-based adhesive resin, the material of the core layer is a polypropylene composition, and the material of the outer layer is a PETG resin composition. The BOPP double-sided heat-sealed film has the advantage of being wear-resistant and has good competitiveness in the packaging field.

[0003] However, in actual use, the inventors found that the BOPP double-sided heat-sealed film prepared by the prior art has poor dust-proof performance and is easy to absorb dust, which needs to be further improved. Summary of the invention

[0004] In order to overcome at least one of the technical problems existing in the prior art, the present invention first provides a BOPP double-sided heat-sealed film and a preparation method thereof.

[0005] The technical solution of the present invention to solve the above technical problems is as follows:

[0006] The present invention first provides a BOPP double-sided heat-sealed film, comprising a core layer and an outer layer.

[0007] The material of the core layer is homopolymer polypropylene resin;

[0008] The material of the outer layer is a polypropylene composition; the polypropylene composition comprises the following components:

[0009] Homopolymer polypropylene resin 80-120 parts; filler 30-50 parts; lubricant 1-3 parts; antioxidant 0.5-2 parts;

[0010] The filler consists of silicon micropowder and graphene.

[0011] The inventors surprisingly found in their research that adding fillers composed of silicon micropowder and graphene to the outer layer material of the BOPP double-sided heat-sealed film can significantly improve the dust-proof performance of the BOPP double-sided heat-sealed film.

[0012] Preferably, the polypropylene composition comprises the following components:

[0013] Homopolymer polypropylene resin 90-110 parts; filler 30-40 parts; lubricant 1-2 parts; antioxidant 0.5-1 part.

[0014] Preferably, the filler is composed of silicon micropowder and graphene in a weight ratio of 3 to 5:1.

[0015] Most preferably, the filler consists of silicon micropowder and graphene in a weight ratio of 4:1.

[0016] Preferably, the filler is a modified filler.

[0017] The modified filler is prepared by the following method:

[0018] (1) taking silicon micropowder and graphene, adding them to water, and then adding ethylenediaminetetramethylenephosphoric acid to obtain a mixed solution;

[0019] (2) Adding metal salt to the mixed solution, stirring for 2 to 5 hours, separating the solid, and drying the solid to obtain the modified filler.

[0020] The inventors found in further research that adding a modified filler obtained by modifying silicon micropowder and graphene by the above method to the outer layer material of the BOPP double-sided heat-sealing film can further improve the dust-proof performance of the BOPP double-sided heat-sealing film compared to adding an unmodified filler composed of silicon micropowder and graphene.

[0021] Preferably, in step (1), the total weight of silicon powder and graphene to the amount of ethylenediaminetetramethylenephosphoric acid and water is 0.8-1.5kg:80-150g:10L.

[0022] Most preferably, in step (1), the total weight of silicon powder and graphene to the amount of ethylenediaminetetramethylenephosphoric acid and water is 1kg:100g:10L.

[0023] Preferably, in step (1), the weight ratio of silicon powder to graphene is 3 to 5:1.

[0024] Most preferably, the weight ratio of silicon powder to graphene in step (1) is 4:1.

[0025] Preferably, in step (2), the ratio of the mixed solution to the metal salt is 10L:100-200g.

[0026] Most preferably, the ratio of the mixed solution to the metal salt in step (2) is 10L:150g.

[0027] Preferably, the metal salt is selected from magnesium chloride or titanium chloride.

[0028] Preferably, the metal salt consists of magnesium chloride and titanium chloride.

[0029] Preferably, the weight ratio of magnesium chloride to titanium chloride is 1 to 3:1.

[0030] Most preferably, the weight ratio of magnesium chloride to titanium chloride is 2:1.

[0031] The inventors found in further research that in step (2) of the preparation method of the modified filler, magnesium chloride and titanium chloride are added simultaneously to modify silicon micropowder and graphene to obtain a modified filler; the degree of improvement in the dustproof performance of the BOPP double-sided heat-sealing film is significantly higher than that of the modified filler obtained by only adding magnesium chloride or titanium chloride to modify silicon micropowder and graphene. In step (2) of the preparation method of the modified filler, magnesium chloride and titanium chloride are added simultaneously to modify silicon micropowder and graphene, which can synergistically improve the dustproof performance of the BOPP double-sided heat-sealing film.

[0032] The present invention also provides a method for preparing the above-mentioned BOPP double-sided heat-sealed film, which comprises the following steps:

[0033] The core layer material and the outer layer material are melt-extruded through an extruder respectively and then converged into the same die head, and then subjected to sheet casting, longitudinal stretching, transverse stretching, pulling and winding treatment to obtain the BOPP double-sided heat-sealed film.

[0034] Beneficial effects: The present invention provides a new method for preparing a BOPP double-sided heat-sealed film; studies have shown that adding fillers composed of silicon micropowder and graphene to the outer layer material of the BOPP double-sided heat-sealed film can significantly improve the dustproof performance of the BOPP double-sided heat-sealed film; and the invention has important application value. DETAILED DESCRIPTION

[0035] The present invention is further explained below in conjunction with specific examples, but the examples do not limit the present invention in any form.

[0036] The homopolymer polypropylene resin used in the following examples is HF409 homopolymer polypropylene produced by Hanwha Total Petrochemical; the remaining raw materials are conventional raw materials that can be purchased or prepared by conventional methods by those skilled in the art.

[0037] Example 1 BOPP double-sided heat-sealed film

[0038] The BOPP double-sided heat-sealed film is composed of two outer layers and a core layer; the thickness of the outer layer is 2 microns; the thickness of the core layer is 30 microns;

[0039] The material of the core layer is homopolymer polypropylene resin;

[0040] The material of the outer layer is a polypropylene composition; the polypropylene composition comprises the following components: 100 parts of homopolymer polypropylene resin; 37 parts of filler; 2 parts of lubricant (calcium stearate); and 1 part of antioxidant (antioxidant 1010).

[0041] The filler is composed of silicon micropowder and graphene in a weight ratio of 4:1.

[0042] The preparation method of BOPP double-sided heat-sealed film is as follows: the core layer material and the outer layer material are melted and extruded through an extruder respectively and then converged into the same die head, and then the BOPP double-sided heat-sealed film is obtained after casting, longitudinal stretching, transverse stretching, pulling and winding.

[0043] Example 2 BOPP double-sided heat-sealed film

[0044] The BOPP double-sided heat-sealed film is composed of two outer layers and a core layer; the thickness of the outer layer is 2 microns; the thickness of the core layer is 30 microns;

[0045] The material of the core layer is homopolymer polypropylene resin;

[0046] The material of the outer layer is a polypropylene composition; the polypropylene composition comprises the following components: 100 parts of homopolymer polypropylene resin; 37 parts of modified filler; 2 parts of lubricant (calcium stearate); and 1 part of antioxidant (antioxidant 1010).

[0047] The modified filler is prepared by the following method:

[0048] (1) taking silicon micropowder and graphene, adding them to water, and then adding ethylenediaminetetramethylenephosphoric acid to obtain a mixed solution; wherein the total weight ratio of silicon micropowder and graphene to ethylenediaminetetramethylenephosphoric acid and water is 1kg:100g:10L; and the weight ratio of silicon micropowder to graphene is 4:1;

[0049] (2) adding a metal salt to the mixed solution, stirring for 3 hours, separating the solid, and drying the solid to obtain the modified filler; wherein the ratio of the mixed solution to the metal salt is 10L:150g; and the metal salt is magnesium chloride.

[0050] The preparation method of BOPP double-sided heat-sealed film is as follows: the core layer material and the outer layer material are melted and extruded through an extruder respectively and then converged into the same die head, and then the BOPP double-sided heat-sealed film is obtained after casting, longitudinal stretching, transverse stretching, pulling and winding.

[0051] Example 3 BOPP double-sided heat-sealed film

[0052] The BOPP double-sided heat-sealed film is composed of two outer layers and a core layer; the thickness of the outer layer is 2 microns; the thickness of the core layer is 30 microns;

[0053] The material of the core layer is homopolymer polypropylene resin;

[0054] The material of the outer layer is a polypropylene composition; the polypropylene composition comprises the following components: 100 parts of homopolymer polypropylene resin; 37 parts of modified filler; 2 parts of lubricant (calcium stearate); and 1 part of antioxidant (antioxidant 1010).

[0055] The modified filler is prepared by the following method:

[0056] (1) taking silicon micropowder and graphene, adding them to water, and then adding ethylenediaminetetramethylenephosphoric acid to obtain a mixed solution; wherein the total weight ratio of silicon micropowder and graphene to ethylenediaminetetramethylenephosphoric acid and water is 1kg:100g:10L; and the weight ratio of silicon micropowder to graphene is 4:1;

[0057] (2) Adding metal salt to the mixed solution, stirring for 3 hours, separating the solid, and drying the solid to obtain the modified filler; wherein the ratio of the mixed solution to the metal salt is 10L:150g; and the metal salt is titanium chloride.

[0058] The preparation method of BOPP double-sided heat-sealed film is as follows: the core layer material and the outer layer material are melted and extruded through an extruder respectively and then converged into the same die head, and then the BOPP double-sided heat-sealed film is obtained after casting, longitudinal stretching, transverse stretching, pulling and winding.

[0059] Example 4 BOPP double-sided heat-sealed film

[0060] The BOPP double-sided heat-sealed film is composed of two outer layers and a core layer; the thickness of the outer layer is 2 microns; the thickness of the core layer is 30 microns;

[0061] The material of the core layer is homopolymer polypropylene resin;

[0062] The material of the outer layer is a polypropylene composition; the polypropylene composition comprises the following components: 100 parts of homopolymer polypropylene resin; 37 parts of modified filler; 2 parts of lubricant (calcium stearate); and 1 part of antioxidant (antioxidant 1010).

[0063] The modified filler is prepared by the following method:

[0064] (1) taking silicon micropowder and graphene, adding them to water, and then adding ethylenediaminetetramethylenephosphoric acid to obtain a mixed solution; wherein the total weight ratio of silicon micropowder and graphene to ethylenediaminetetramethylenephosphoric acid and water is 1kg:100g:10L; and the weight ratio of silicon micropowder to graphene is 4:1;

[0065] (2) adding metal salt to the mixed solution, stirring for 3 hours, separating the solid, and drying the solid to obtain the modified filler; wherein the ratio of the mixed solution to the metal salt is 10L:150g; and the metal salt is composed of magnesium chloride and titanium chloride in a weight ratio of 2:1.

[0066] The preparation method of BOPP double-sided heat-sealed film is as follows: the core layer material and the outer layer material are melted and extruded through an extruder respectively and then converged into the same die head, and then the BOPP double-sided heat-sealed film is obtained after casting, longitudinal stretching, transverse stretching, pulling and winding.

[0067] Comparative Example 1 BOPP double-sided heat-sealed film

[0068] The BOPP double-sided heat-sealed film is composed of two outer layers and a core layer; the thickness of the outer layer is 2 microns; the thickness of the core layer is 30 microns;

[0069] The material of the core layer is homopolymer polypropylene resin;

[0070] The material of the outer layer is a polypropylene composition; the polypropylene composition comprises the following components: 100 parts of homopolymer polypropylene resin; 2 parts of lubricant (calcium stearate); and 1 part of antioxidant (antioxidant 1010).

[0071] The preparation method of BOPP double-sided heat-sealed film is as follows: the core layer material and the outer layer material are melted and extruded through an extruder respectively and then converged into the same die head, and then the BOPP double-sided heat-sealed film is obtained after casting, longitudinal stretching, transverse stretching, pulling and winding.

[0072] Experimental Example 1 Dust Test

[0073] Take 100g of talcum powder and place it in a box with a length of 50cm, a width of 30cm and a height of 50cm with a blower at the bottom, and hang the BOPP double-sided heat-sealed film to be tested with a length of 10cm and a width of 10cm on the top of the box; turn on the blower to fill the box with talcum powder, and weigh the weight of the BOPP double-sided heat-sealed film to be tested after 12 hours, and calculate the dust adsorption amount; dust adsorption amount = weight of BOPP double-sided heat-sealed film after adsorption - weight of BOPP double-sided heat-sealed film before adsorption; the test results are shown in Table 1.

[0074] The BOPP double-sided heat-sealed film to be tested is the BOPP double-sided heat-sealed film prepared in Examples 1 to 4 and Comparative Example 1.

[0075] Table 1. Dustproof test results of BOPP double-sided heat-sealed film of the present invention

[0076] Dust adsorption capacity BOPP double-sided heat-sealed film prepared in Example 1 318mg BOPP double-sided heat-sealed film prepared in Example 2 264mg BOPP double-sided heat-sealed film prepared in Example 3 239mg BOPP double-sided heat-sealed film prepared in Example 4 157mg BOPP double-sided heat-sealed film prepared in Comparative Example 1 543mg

[0077] It can be seen from the experimental results in Table 1 that the dust adsorption amount of the BOPP double-sided heat-sealed film prepared in Example 1 is significantly smaller than that of the BOPP double-sided heat-sealed film prepared in Comparative Example 1; this indicates that adding a filler composed of silicon micropowder and graphene to the outer layer material of the BOPP double-sided heat-sealed film can significantly improve the dust-proof performance of the BOPP double-sided heat-sealed film.

[0078] It can be seen from the experimental results in Table 1 that the dust adsorption amount of the BOPP double-sided heat-sealed film prepared in Examples 2 and 3 is further less than that of the BOPP double-sided heat-sealed film prepared in Example 1; this indicates that adding the modified filler obtained by modifying silicon micropowder and graphene by the method of the present invention to the outer layer material of the BOPP double-sided heat-sealed film can further improve the dust-proof performance of the BOPP double-sided heat-sealed film compared with adding the unmodified filler composed of silicon micropowder and graphene.

[0079] From the experimental results in Table 1, it can be seen that the dust adsorption amount of the BOPP double-sided heat-seal film prepared in Example 4 is further significantly less than that of the BOPP double-sided heat-seal films prepared in Examples 2 and 3; this shows that: in step (2) of the preparation method of the modified filler, magnesium chloride and titanium chloride are added simultaneously to modify silicon micropowder and graphene to obtain a modified filler; the degree of improvement in the dust-proof performance of the BOPP double-sided heat-seal film is significantly higher than that of the modified filler obtained by only adding magnesium chloride or titanium chloride to modify silicon micropowder and graphene. In step (2) of the preparation method of the modified filler, magnesium chloride and titanium chloride are added simultaneously to modify silicon micropowder and graphene, which can synergistically improve the dust-proof performance of the BOPP double-sided heat-seal film.

Claims

1. A BOPP double-sided heat-sealed film, comprising a core layer and an outer layer, characterized in that: The material of the core layer is homopolymer polypropylene resin; The material of the outer layer is a polypropylene composition; the polypropylene composition comprises the following components: Homopolymer polypropylene resin 80-120 parts; filler 30-50 parts; lubricant 1-3 parts; antioxidant 0.5-2 parts; The filler consists of silicon micropowder and graphene.

2. The BOPP double-sided heat-sealed film according to claim 1, characterized in that: The polypropylene composition comprises the following components: Homopolymer polypropylene resin 90-110 parts; filler 30-40 parts; lubricant 1-2 parts; antioxidant 0.5-1 part.

3. The BOPP double-sided heat-sealed film according to claim 1, characterized in that: The filler is composed of silicon micropowder and graphene in a weight ratio of 3 to 5:

1. Most preferably, the filler consists of silicon micropowder and graphene in a weight ratio of 4:

1.

4. The BOPP double-sided heat-sealed film according to claim 1, characterized in that: The filler is a modified filler. The modified filler is prepared by the following method: (1) taking silicon micropowder and graphene, adding them to water, and then adding ethylenediaminetetramethylenephosphoric acid to obtain a mixed solution; (2) Adding metal salt to the mixed solution, stirring for 2 to 5 hours, separating the solid, and drying the solid to obtain the modified filler.

5. The BOPP double-sided heat-sealed film according to claim 4, characterized in that: In step (1), the total weight of silicon powder and graphene, ethylenediaminetetramethylenephosphoric acid and water are in a ratio of 0.8-1.5kg:80-150g:10L. Most preferably, in step (1), the total weight of silicon powder and graphene to the amount of ethylenediaminetetramethylenephosphoric acid and water is 1kg:100g:10L.

6. The BOPP double-sided heat-sealed film according to claim 4, characterized in that: In step (2), the ratio of the mixed solution to the metal salt is 10L:100-200g; Most preferably, the ratio of the mixed solution to the metal salt in step (2) is 10L:150g.

7. The BOPP double-sided heat-sealed film according to claim 4, characterized in that: The metal salt is selected from magnesium chloride or titanium chloride.

8. The BOPP double-sided heat-sealed film according to claim 4, characterized in that: The metal salt consists of magnesium chloride and titanium chloride.

9. The BOPP double-sided heat-sealed film according to claim 8, characterized in that: The weight ratio of magnesium chloride to titanium chloride is 1 to 3:1; Most preferably, the weight ratio of magnesium chloride to titanium chloride is 2:

1.

10. The method for preparing the BOPP double-sided heat-sealable film according to any one of claims 1 to 8, characterized in that: The following steps are included: The core layer material and the outer layer material are melt-extruded through an extruder respectively and then converged into the same die head, and then subjected to sheet casting, longitudinal stretching, transverse stretching, pulling and winding treatment to obtain the BOPP double-sided heat-sealed film.

Citation Information

Patent Citations

  • BOPP film for leather printing transfer and manufacturing method thereof

    CN101774290A

  • High-weather-resistance biaxially oriented polypropylene bag preparing film and preparation process thereof

    CN106273971A

  • BOPP double-sided heat-sealing film and preparation method thereof

    CN110065281A

  • Novel outer packing BOPP composite film structure easy to open and application of novel outer packing BOPP composite film structure

    CN115946971A