Food packaging film for high-temperature cooking, packaging bag and preparation method

By using the composite technology of the barrier surface layer and polyethylene layer in the high-temperature cooking packaging film, the problem of glue affecting food safety and insufficient barrier performance in the existing technology is solved, better barrier performance and adaptability are achieved, and the shelf life of food is extended .

CN118876546AActive Publication Date: 2024-11-01GREEN PACKAGING MATERIAL (JIANGYIN) CO LTD

Patent Information

Application Number
CN202410794206.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-11-01
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

The use of solvent-based glue in the production process of existing high-temperature cooking packaging films affects food safety, and poor barrier performance leads to a short shelf life of the packaging.

Method used

Using a laminated structure of the barrier surface layer, the first barrier layer, the second barrier layer and the barrier heat sealing layer, the nylon layer is coextruded with the polyethylene layer composited with mLLDPE and HDPE to improve the barrier performance of the packaging film and adapt to different soft and hard Package of degree.

Benefits of technology

It improves the barrier properties of the packaging film, makes it soft and resistant to puncture, and adapts to irregular packaging, extending the shelf life of food.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004900976220000091
    Figure BDA0004900976220000091
  • Figure BDA0004900976220000101
    Figure BDA0004900976220000101
Patent Text Reader

Abstract

The invention discloses a food packaging film for high-temperature cooking, which is a co-extruded film and comprises a barrier surface layer, a first bonding layer, a high-temperature-resistant layer, a second bonding layer, a first barrier layer, a third bonding layer, a second barrier layer and a barrier heat-sealing layer which are sequentially stacked, the barrier surface layer mainly comprises nylon and amorphous nylon; the first barrier layer mainly comprises nylon; the second barrier layer is mainly composed of mLLDPE and HDPE; the barrier heat sealing layer mainly comprises mLLDPE, HDPE (high-density polyethylene) and an anti-blocking agent. The food packaging film for high-temperature cooking is reasonable in structure, the barrier property of the packaging film is improved through a laminated structure of the barrier surface layer, the first barrier layer, the second barrier layer and the barrier heat-sealing layer, and the obtained packaging film is soft and puncture-resistant through co-extrusion compounding of the nylon layer and the polyethylene layer compounded by the mLLDPE and the HDPE; further, the packaging material is suitable for irregular packaging materials with different hardness, and the barrier property is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of packaging films, and in particular to a food packaging film and a packaging bag for high-temperature cooking, and a preparation method thereof. Background Art

[0002] Common high-temperature cooking packaging products on the market are composite films of nylon film and PP film (polypropylene), which need to be compounded with high-temperature resistant glue. The production process is complicated and long. Glue is required in the compounding process. Generally, the glue is solvent-based, which will have a negative impact on food safety. Existing high-temperature cooking packaging products also have the problem of poor barrier properties, which can easily lead to a short shelf life of the inner packaging.

[0003] Therefore, it is necessary to improve packaging film and production in the prior art. Summary of the invention

[0004] One of the purposes of the present invention is to overcome the defects existing in the prior art and provide a food packaging film for high-temperature cooking. The barrier properties of the packaging film are improved by a laminated structure of a barrier surface layer, a first barrier layer, a second barrier layer and a barrier heat-sealing layer. The nylon layer is co-extruded with a polyethylene layer composited with mLLDPE and HDPE. The obtained packaging film is not only soft and puncture-resistant, but also adaptable to irregular and different soft and hard packaging materials, and has excellent barrier properties.

[0005] In order to achieve the above-mentioned process effect, the technical solution of the present invention is as follows: a high-temperature cooking food packaging film is a co-extruded film, comprising a barrier surface layer, a first adhesive layer, a high-temperature resistant layer, a second adhesive layer, a first barrier layer, a third adhesive layer, a second barrier layer and a barrier heat-sealing layer stacked in sequence;

[0006] The barrier surface layer is mainly composed of nylon and amorphous nylon;

[0007] The first barrier layer is mainly composed of nylon;

[0008] The main components of the second barrier layer include mLLDPE and HDPE;

[0009] The main components of the barrier heat seal layer include mLLDPE, HDPE and an opening agent.

[0010] The preferred technical solution is: the high temperature resistant layer comprises a layer A and a layer B which are compounded from the outside to the inside;

[0011] The main components of the A layer and the B layer include mLLDPE and PP;

[0012] The mass ratio of mLLDPE to PP in the A layer is (60-75): (25-40);

[0013] The mass ratio of mLLDPE to PP in the B layer is (60-75):(25-40).

[0014] Furthermore, the mass ratio of mLLDPE to PP in layer A is (65-75): (25-35); the mass ratio of mLLDPE to PP in layer B is (65-75): (25-35). Furthermore, the mass ratio of mLLDPE to PP in layer A is (67-72): (28-33); the mass ratio of mLLDPE to PP in layer B is (67-72): (28-33).

[0015] The preferred technical solution is: the main components of the A layer and / or the B layer also include CBC accounting for 10% to 20% of the total mass of the high temperature resistant layer; the main components of the second barrier layer also include CBC. Further, the composition of the A layer includes CBC.

[0016] The preferred technical solution is: the first adhesive layer includes mLLDPE and maleic anhydride modified high-density polyethylene adhesive, and the mass ratio of mLLDPE and maleic anhydride modified high-density polyethylene adhesive in the first adhesive layer is (1-2.4): 1. Furthermore, the mass ratio of mLLDPE and maleic anhydride modified high-density polyethylene adhesive in the first adhesive layer is (1-2): 1.

[0017] The preferred technical solution is: the main components of the barrier surface layer include 105-115 parts of nylon and 15-25 parts of amorphous nylon, calculated by weight;

[0018] The second barrier layer mainly comprises 60-70 parts of mLLDPE, 20-30 parts of HDPE and 7-13 parts of CBC;

[0019] The main components of the barrier heat seal layer include 70-80 parts of mLLDPE, 20-30 parts of HDPE and 4-6 parts of an opening agent.

[0020] Furthermore, the main components of the barrier surface layer include 110-115 parts of nylon and 18-22 parts of amorphous nylon. Furthermore, the main components of the barrier surface layer include 110-113 parts of nylon and 19-22 parts of amorphous nylon.

[0021] Furthermore, the second barrier layer mainly comprises 62-68 parts of mLLDPE, 22-28 parts of HDPE and 8-12 parts of CBC.

[0022] Furthermore, the main components of the barrier heat seal layer include 72-80 parts of mLLDPE, 20-28 parts of HDPE and 4-6 parts of an opening agent.

[0023] The preferred technical solution is: the thickness ratio of the A layer and the B layer is (1-2.2):1, the thickness of the high temperature resistant layer accounts for 22%-32% of the total film thickness of the packaging film, and the total film thickness of the packaging film is 90-200 μm.

[0024] The preferred technical solution is: the density of mLLDPE in the high temperature resistant layer, the second barrier layer and the barrier heat seal layer is 0.930-0.940 g / cm 3 The melt index is 0.45-0.56 g / 10 min; the density of PP in the high temperature resistant layer is 0.880-0.950 g / cm 3 The melt index is 1.4-2.0 g / 10 min; the density of HDPE in the second barrier layer and the barrier heat seal layer is 0.945-0.955 g / cm 3 , the melt index is 0.9-1.3 g / 10 min; the density of the CBC is 0.92-0.95 g / cm 3 , the melt index is 1 to 3 g / 10 min.

[0025] The preferred technical solution is: the brand of mLLDPE in the high temperature resistant layer, the second barrier layer and the barrier heat seal layer is 3505MC; the brand of PP in the high temperature resistant layer is RB707CF; the brand of HDPE in the second barrier layer is HD3355F, and the brand of CBC is ViviOn8210XT.

[0026] The second object of the present invention is to overcome the defects existing in the prior art and provide a high-temperature cooking food packaging bag, comprising a first bag surface, the first bag surface is the above-mentioned high-temperature cooking food packaging film, and the barrier heat sealing layer is the inner surface of the first bag surface.

[0027] The third object of the present invention is to overcome the defects existing in the prior art and provide a method for preparing a high-temperature cooking food packaging film, wherein the high-temperature cooking food packaging film is the above-mentioned high-temperature cooking food packaging film, the extrusion temperature of the barrier surface layer is 260-270°C, the extrusion temperature of the first adhesive layer is 230-240°C, the extrusion temperature of the high temperature resistant layer is 220-230°C, the extrusion temperature of the second adhesive layer is 230-240°C, the extrusion temperature of the first barrier layer is 260-270°C, the extrusion temperature of the third adhesive layer is 230-240°C, the extrusion temperature of the second barrier layer is 230-240°C, and the extrusion temperature of the barrier heat sealing layer is 220-230°C.

[0028] The advantages and beneficial effects of the present invention are:

[0029] The high-temperature cooking food packaging film has a reasonable structure. The barrier properties of the packaging film are improved through the laminated structure of the barrier surface layer, the first barrier layer, the second barrier layer and the barrier heat sealing layer. The nylon layer is co-extruded with the polyethylene layer of mLLDPE and HDPE. The obtained packaging film is not only soft and puncture-resistant, but also adaptable to irregular and different hardness packaging, and has excellent barrier properties. DETAILED DESCRIPTION

[0030] The specific implementation of the present invention is further described below in conjunction with the examples. The following examples are only used to more clearly illustrate the technical solutions of the present invention, and cannot be used to limit the protection scope of the present invention.

[0031] definition

[0032] In the present disclosure, the term "mLLDPE" refers to a polymer prepared by ethylene polymerization using a metallocene coordination compound as a catalyst.

[0033] In this disclosure, the term "HDPE" refers to high-density polyethylene, which is polymerized by ethylene gas under high temperature and pressure by a catalyst. The molecular chain is basically linear, so there are no or very few branches on its main chain.

[0034] In this disclosure, the term "PP" refers to polypropylene, which is a thermoplastic resin obtained by the addition polymerization of propylene monomers. The molecular chain of polypropylene is composed of propylene monomer units connected by carbon-carbon single bonds, and each propylene unit contributes a methyl (-CH3) side group on the molecular chain. According to the arrangement of methyl groups on the molecular chain, polypropylene can be divided into three types: isotactic polypropylene, atactic polypropylene and syndiotactic polypropylene.

[0035] In the present disclosure, the term "CBC" refers to a novel cyclic block copolymer prepared by fully hydrogenating styrene and conjugated olefin copolymers using a special high-efficiency catalyst.

[0036] model

[0037] Nylon is produced by Nantong Weiming New Materials Co., Ltd., with the trade name J36TFE;

[0038] Amorphous nylon is produced by EMS of Switzerland with the trade name G21;

[0039] Maleic anhydride modified high-density polyethylene adhesive is produced by Guangzhou Synthetic New Materials Company, with the trade name HS3-405Z;

[0040] The cyclic block copolymer (CBC) was purchased from Taiwan Polymer Chemicals Co., Ltd., China, with the trade name ViviOn 8210XT.

[0041] The opening agent is produced by Hong Kong Huayi Company and its trade number is SF109.

[0042] High temperature cooking food packaging film

[0043] The thickness of the barrier surface layer accounts for 9% to 11% of the total thickness of the packaging film, the thickness of the first adhesive layer, the second adhesive layer and the third adhesive layer each account for 7% to 9% of the total thickness of the packaging film, the thickness of the high temperature resistant layer accounts for 22% to 32% of the total thickness of the packaging film, the thickness of the first barrier layer accounts for 9% to 11% of the total thickness of the packaging film, the thickness of the second barrier layer accounts for 8% to 11% of the total thickness of the packaging film, and the thickness of the barrier heat sealing layer accounts for 17% to 25% of the total thickness of the packaging film.

[0044] Barrier surface

[0045] Amorphous nylon refers to semi-crystalline-crystalline thermoplastic materials. It includes nylon and amorphous nylon; further, nylon is homopolymer nylon PA6. Homopolymer nylon has a high melting point and thermal stability, which enables it to maintain good physical and mechanical properties under high-temperature cooking conditions, and is not prone to thermal deformation or degradation, thereby ensuring the integrity of the packaging; it also has higher tensile strength and rigidity, which helps the packaging material remain tough during high-temperature treatment and subsequent logistics processes, reducing the risk of breakage; it has good resistance to grease, acidic and alkaline substances within a certain range, which is particularly important for food packaging that requires high-temperature cooking, and can effectively prevent the packaging material from chemically reacting or being corroded when it comes into contact with food contents; it usually provides good oxygen and water vapor barrier properties, which helps to extend the shelf life of food and maintain the freshness of food.

[0046] The barrier surface layer is compounded with amorphous nylon and PA6 to improve the transparency of the packaging film. More PA6 can improve the strength and gas barrier performance; less PA6 can damage the mechanical strength of the packaging film.

[0047] High temperature resistant layer

[0048] It includes layer A and layer B that are compounded from the outside to the inside, and the main components of layer A and layer B include mLLDPE and PP. Among them, mLLDPE helps to provide clarity and gloss, making the appearance of the product in the package more attractive; mLLDPE gives the packaging film better softness and ductility, making the packaging easier to adapt to changes in the shape of the contents, especially when processed at high temperatures, it can resist changes in internal pressure and reduce the risk of rupture. The PP component ensures the structural stability and shape retention of the packaging film during high-temperature boiling or steaming. It can withstand high temperatures without melting or deformation; PP has excellent impact resistance, which can further enhance the packaging film's resistance to rupture and extend its service life. The combined use of mLLDPE and PP can increase the tear strength and puncture resistance of the packaging film while maintaining good flexibility. Excessive addition of mLLDPE has a negative effect on the temperature resistance and rigidity of the packaging film. CBC materials generally have good heat resistance, which means that during high-temperature cooking or heating, their barrier properties will not drop as quickly as some plastics, maintaining the integrity of the package and preventing contamination of the contents; and their gas barrier and water vapor barrier properties are excellent; CBC's high transparency and low fluorescence properties, combined with the transparency of mLLDPE, can produce packaging or optical products that are both transparent and have low visual interference.

[0049] Second barrier layer and barrier heat seal layer

[0050] The main components of the second barrier layer include mLLDPE and HDPE; the main components of the second barrier layer include mLLDPE, HDPE and CBC. The main components of the barrier heat seal layer include mLLDPE, HDPE and an opening agent. Among them, HDPE has good low temperature resistance, high mechanical strength and certain toughness, which can enhance the physical strength of the film, such as improving tensile strength and abrasion resistance, making the packaging more durable and not easy to break; HDPE has excellent water vapor resistance, which can effectively prevent moisture penetration and keep the contents of the package fresh and dry. HDPE is suitable as a heat seal layer for cooking bags due to its good heat resistance; and the addition of mLLDPE can further enhance the sealing strength and heat resistance of the heat seal area, ensure the sealing reliability of the packaging during high-temperature cooking, and reduce the risk of leakage. mLLDPE complements the high strength and rigidity of HDPE with its high toughness, low brittleness and good impact resistance, while CBC may provide additional strength and elasticity through its unique structure. As a high-performance material, CBC may have better gas and water vapor barrier properties than traditional PE materials. Combining it with mLLDPE and HDPE can enhance the aroma and freshness preservation capabilities of packaging or coatings while maintaining the good mechanical properties of the material.

[0051] Example 1

[0052] The food packaging film for high-temperature cooking is a co-extruded film, including a barrier surface layer, a first adhesive layer, a high-temperature resistant layer, a second adhesive layer, a first barrier layer, a third adhesive layer, a second barrier layer and a barrier heat-sealing layer stacked in sequence; wherein the high-temperature resistant layer includes layer A and layer B composited from the outside to the inside.

[0053] In terms of weight, the composition of the barrier surface layer is 112.5 parts of nylon and 20 parts of amorphous nylon; the composition of mLLDPE in layer A is 70 parts and PP is 30 parts; the composition of mLLDPE in layer B is 70 parts and PP is 30 parts; the composition of the first barrier layer is 100 parts of nylon; the composition of the second barrier layer is 70 parts of mLLDPE and 30 parts of HDPE; the composition of the barrier heat sealing layer is 75 parts of mLLDPE, 25 parts of HDPE, and 5 parts of anti-blocking agent; the first adhesive layer, the second adhesive layer and the third adhesive layer all include 50 parts of mLLDPE (3505MC) and 50 parts of maleic anhydride modified high-density polyethylene adhesive.

[0054] Among them, the total film thickness of the packaging film is 150μm, the thickness of the barrier surface layer is 15μm, the thickness of the first adhesive layer, the second adhesive layer and the third adhesive layer are all 12μm, the thickness of the high temperature resistant layer is 42μm, the thickness of layer A is 28.5μm, the thickness of layer B is 13.5μm, the thickness of the first barrier layer is 14.25μm, the thickness of the second barrier layer is 15.75μm, and the thickness of the barrier heat sealing layer is 27μm.

[0055] The extrusion temperature of the barrier surface layer is 220℃, 260℃, 265℃, 265℃, 265℃, 265℃, 265℃;

[0056] The extrusion temperature of the first adhesive layer is 80°C, 235°C, 235°C, 235°C, 235°C, 235°C, 235°C;

[0057] The extrusion temperature of layer A is 80℃, 225℃, 225℃, 225℃, 225℃, 225℃, 225℃;

[0058] The extrusion temperature of layer B is 80℃, 225℃, 225℃, 225℃, 225℃, 225℃, 225℃;

[0059] The second adhesive layer extrusion temperature is 80°C, 235°C, 235°C, 235°C, 235°C, 235°C, 235°C;

[0060] The extrusion temperatures of the first barrier layer are 195°C, 265°C, 265°C, 265°C, 265°C, 265°C, 265°C;

[0061] The extrusion temperature of the third adhesive layer is 80°C, 235°C, 235°C, 235°C, 235°C, 235°C, 235°C;

[0062] The second barrier layer extrusion temperature is 80°C, 235°C, 235°C, 235°C, 235°C, 235°C, 235°C;

[0063] The extrusion temperatures of the barrier heat seal layer are 80°C, 225°C, 225°C, 225°C, 225°C, 225°C, and 225°C.

[0064] Example 2

[0065] Example 2 is based on Example 1, except that the A layer contains 70 parts of mLLDPE, 30 parts of PP and 30 parts of CBC, and the second barrier layer contains 65 parts of mLLDPE, 25 parts of HDPE and 10 parts of CBC. The other layers remain unchanged.

[0066] Example 3

[0067] Example 3 is based on Example 1, except that the A layer contains 70 parts of mLLDPE, 30 parts of PP and 30 parts of CBC, while the other layers remain unchanged.

[0068] Example 4

[0069] Example 4 is based on Example 1, except that the second barrier layer is composed of 65 parts of mLLDPE, 25 parts of HDPE and 10 parts of CBC, while the other layers remain unchanged.

[0070] Example 5

[0071] Example 5 is based on Example 2, except that the high temperature resistant layer includes a layer A and a layer B which are compounded from the outside to the inside, wherein the composition of the layer A is mLLDPE, and the composition of the layer B is PP. The other layers remain unchanged.

[0072] Example 6

[0073] Example 6 is based on Example 2, except that, the total film thickness of the packaging film is 90 μm, the thickness of the barrier surface layer is 8.55 μm, the thickness of the first adhesive layer, the second adhesive layer and the third adhesive layer are all 7.2 μm, the thickness of the high temperature resistant layer is 25.2 μm, the thickness of layer A is 18 μm, the thickness of layer B is 7.2 μm, the thickness of the first barrier layer is 8.55 μm, the thickness of the second barrier layer is 7.1 μm, and the thickness of the barrier heat sealing layer is 19 μm.

[0074] Example 7

[0075] Example 7 is based on Example 2, except that the total film thickness of the packaging film remains unchanged, the thickness of the second barrier layer is 27 μm, the thickness of the barrier heat seal layer is 15.75 μm, and the thickness of other layers remains unchanged.

[0076] Comparative Example 1

[0077] Comparative Example 1 is based on Example 2, except that the second barrier layer does not contain HDPE, and the composition of the second barrier layer is 90 parts of mLLDPE and 10 parts of CBC.

[0078] Sample testing method:

[0079] 1. Determination of tensile strength and elongation at break: according to the test standard

[0080] GB / T1040.3-2006;

[0081] 2. Water vapor transmission rate determination: according to the test standard GB / T1037-1988;

[0082] 3. Oxygen permeability measurement: according to the test standard GB / T1038-2000;

[0083] 4. Transmittance determination: according to the test standard GB / T2410-2008;

[0084] 5. Heat seal strength determination: according to the test standard QB / T2358-1998;

[0085] 6. Heat resistance determination: according to the test standard GB / T10004-2008.

[0086] 7. Bag drop test: Pack 1 kg of rice in the packaging bags made of the packaging films of the embodiment and the comparative example as samples, and then drop the bottom and two sides of the bags of the samples freely from a height of 1 meter. Each group of tests is tested three times to observe whether there is any cracking.

[0087] 9. Freezing test: 1 kg of water was packed in the packaging bags made of the packaging films of the embodiments and comparative examples as a sample, and frozen at -18°C. The integrity of the packaging bags was then taken out and observed for leakage, rupture, and changes in the quality of the packaging contents.

[0088] The test results of the packaging bags of the embodiments and comparative examples are as follows:

[0089]

[0090]

[0091] Compared with Example 2, Example 1 has inferior barrier performance.

[0092] Compared with Example 2, the barrier properties of Example 3 and Example 4 are inferior.

[0093] Compared with Example 2, Example 5 has a higher hardness of the packaging film. This is difficult to process in practice and may lead to an unstable layer structure of the packaging film, which has a negative impact on mechanical properties and heat resistance. The test found that if the composition of layer A is PP and the composition of layer B is mLLDPE, the thickness of layer A is greater than that of layer B, resulting in an increase in the hardness of the packaging film, and poor results in the bag drop test and the freezing test.

[0094] In Example 7, compared with Example 2, the thickness of the second barrier layer is increased, and the thickness of the barrier heat seal layer is too small, which has a negative impact on the heat seal strength and barrier performance, and the heat seal portion of the packaging film peels off in the bag drop test.

[0095] Comparative Example 1 Compared with Example 2, the barrier property of the packaging film obtained by combining the second barrier layer of HDPE, mLLDPE and CBC is better.

[0096] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A food packaging film for high temperature cooking, which is a co-extruded film, characterized in that: It includes a barrier surface layer, a first adhesive layer, a high temperature resistant layer, a second adhesive layer, a first barrier layer, a third adhesive layer, a second barrier layer and a barrier heat seal layer stacked in sequence; The barrier surface layer is mainly composed of nylon and amorphous nylon; The first barrier layer is mainly composed of nylon; The main components of the second barrier layer include mLLDPE and HDPE; The main components of the barrier heat seal layer include mLLDPE, HDPE and an opening agent.

2. The high temperature cooking food packaging film according to claim 1, characterized in that: The high temperature resistant layer comprises a layer A and a layer B which are compounded from the outside to the inside; The main components of the A layer and the B layer include mLLDPE and PP; The mass ratio of mLLDPE to PP in the A layer is (60-75): (25-40); The mass ratio of mLLDPE to PP in the B layer is (60-75):(25-40).

3. The high temperature cooking food packaging film according to claim 2, characterized in that: The main components of the A layer and / or the B layer also include CBC which accounts for 10% to 20% of the total mass of the high temperature resistant layer; the main components of the second barrier layer also include CBC.

4. The high temperature cooking food packaging film according to claim 1 or 2, characterized in that: The first adhesive layer comprises mLLDPE and maleic anhydride modified high-density polyethylene adhesive, and the mass ratio of mLLDPE and maleic anhydride modified high-density polyethylene adhesive in the first adhesive layer is (1-2.4):

1.

5. The high temperature cooking food packaging film according to claim 3, characterized in that: The main components of the barrier surface layer include 105-115 parts of nylon and 15-25 parts of amorphous nylon by weight; The second barrier layer mainly comprises 60-70 parts of mLLDPE, 20-30 parts of HDPE and 7-13 parts of CBC; The main components of the barrier heat seal layer include 70-80 parts of mLLDPE, 20-30 parts of HDPE and 4-6 parts of an opening agent.

6. The high temperature cooking food packaging film according to claim 3, characterized in that: The thickness ratio of the A layer to the B layer is (1-2.2):1, the thickness of the high temperature resistant layer accounts for 22%-32% of the total film thickness of the packaging film, and the total film thickness of the packaging film is 90-200 μm.

7. The high temperature cooking food packaging film according to claim 3, characterized in that: The density of mLLDPE in the high temperature resistant layer, the second barrier layer and the barrier heat seal layer is 0.930-0.940 g / cm 3 The melt index is 0.45-0.56 g / 10 min; the density of PP in the high temperature resistant layer is 0.880-0.950 g / cm 3 The melt index is 1.4-2.0 g / 10 min; the density of HDPE in the second barrier layer and the barrier heat seal layer is 0.945-0.955 g / cm 3 , the melt index is 0.9-1.3 g / 10 min; the density of the CBC is 0.92-0.95 g / cm 3 , the melt index is 1 to 3 g / 10 min.

8. The high temperature cooking food packaging film according to claim 3 or 7, characterized in that: The grade of mLLDPE in the high temperature resistant layer, the second barrier layer and the barrier heat sealing layer is 3505MC; the grade of PP in the high temperature resistant layer is RB707CF; the grade of HDPE in the second barrier layer is HD3355F, and the grade of CBC is ViviOn8210XT.

9. A food packaging bag for high temperature cooking, comprising a first bag surface, characterized in that: The first bag surface is the high-temperature cooking food packaging film according to any one of claims 1 to 8, and the barrier heat-sealing layer is the inner surface of the first bag surface.

10. A method for preparing a food packaging film for high temperature cooking, characterized in that: The high-temperature cooking food packaging film is the high-temperature cooking food packaging film according to any one of claims 1 to 8, the extrusion temperature of the barrier surface layer is 260-270°C, the extrusion temperature of the first adhesive layer is 230-240°C, the extrusion temperature of the high-temperature resistant layer is 220-230°C, the extrusion temperature of the second adhesive layer is 230-240°C, the extrusion temperature of the first barrier layer is 260-270°C, the extrusion temperature of the third adhesive layer is 230-240°C, the extrusion temperature of the second barrier layer is 230-240°C, and the extrusion temperature of the barrier heat sealing layer is 220-230°C.

Citation Information

Patent Citations

  • High-temperature-resistant boiling packaging film with three-layer structure

    CN103707601A

  • Cold-drawing film and preparation method thereof

    CN106945367A

  • High-temperature-resistant PE film

    CN114013143A

  • Preparation method of puncture-resistant tear-resistant high-transparency PE / POE / CBC blended cast film composition

    CN116834348A

  • Cooking-resistant packaging bag

    CN219635928U

Cited By

  • High-temperature cooking packaging bag

    CN120040875A