Hard sheet, preparation method thereof and ultrathin fiberboard

By combining the hot pressing of modified melamine formaldehyde resin and water-based hot melt adhesive with glass fiber non-woven fabric and glass cloth, the problems of excessive formaldehyde, high water absorption and expansion rate and complex processes of ultra-thin fiberboard are solved, and high strength and low Preparation of ultra-thin fiberboard that absorbs water and is beautiful.

CN118876572AActive Publication Date: 2024-11-01GUANGDONG NATURE HOME FURNISHING TECH RES CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410994299.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-01
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The existing ultra-thin fiberboards have problems such as excessive formaldehyde, high water absorption thickness expansion rate, complex process and poor aesthetics.

Method used

Modified low formaldehyde melamine formaldehyde resin and water-based hot melt adhesive are used as adhesives, combined with glass fiber non-woven fabrics and glass fabrics, and hot-pressing is carried out through a specific combination to form a hard sheet and be combined with plywood base. The material, the printing layer and the wear-resistant layer were heat-pressed in order from bottom to top to obtain ultra-thin fiberboard.

Benefits of technology

The formaldehyde emission reduction, the water absorption thickness expansion rate is controlled below 5%, the surface is smooth and flat, the internal bonding strength reaches more than 1.2MPa, meets the Class II plywood standards, and the process is simplified and the aesthetics are improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention is suitable for the technical field of materials, and provides a hard sheet and a preparation method thereof and an ultrathin fiberboard. Specially-made melamine formaldehyde resin and water-based hot melt adhesive are used as adhesive main bodies, glass fiber non-woven fabric and glass cloth are used as base materials, and the ultra-thin fiberboard is prepared through the steps that the adhesive main bodies are prepared; the glass fiber non-woven fabric and the glass cloth are soaked in the adhesive and then dried to form the prepregs, the prepregs are pressed into the board according to a specific combination mode, and the obtained hard sheet is more close to transparent color in color, better in attractiveness, low in water absorption thickness swelling rate and good in water absorption performance. Meanwhile, the glass cloth is used as balance, so that plate cracking caused by inconsistent thermal expansion coefficients among different layers can be avoided, and the scheme of mixing the glass fiber non-woven fabric and the glass cloth is adopted, so that the specific surface area is small, the glue consumption can be reduced, and the formaldehyde emission is low. The internal bonding strength of the prepared ultrathin fiberboard can reach 1.2 MPa or above, dipping and stripping can reach the standard of class II plywood, and the thickness swelling rate of 24-hour water absorption is lower than 5%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of material technology, and in particular relates to a hard sheet material and a preparation method thereof, and an ultra-thin fiberboard. Background Art

[0002] At present, there are three main types of flooring substrates on the market: fiberboard (wood fibers bonded together with glue), plywood (wood veneer bonded together with glue) and solid wood. Among them, plywood is popular among consumers due to its high cost performance. After the plywood substrate is prepared, a layer of impregnated paper impregnated with melamine glue is attached to the surface. The impregnated paper is in a semi-cured state and then cured by hot pressing again at high temperature and high pressure. Since the surface flatness of the plywood substrate is not enough and direct pressing will produce ribs and affect the overall appearance, it is necessary to press the impregnated paper and ultra-thin fiberboard (about 1mm) first, and then use glue to bond the ultra-thin fiberboard and plywood substrate together.

[0003] However, the use of existing ultra-thin fiberboards has the following disadvantages: ① Since urea-formaldehyde glue or phenol-formaldehyde glue containing formaldehyde is mainly used, it is easy to cause the overall formaldehyde content of the board to exceed the standard; ② Because ultra-thin fiberboard is a fiberboard after all, it is easy to cause the water absorption thickness expansion rate to be too high after contacting water, affecting the overall performance indicators; ③ When observed from the side, a layer of brown fiberboard is added in the middle of the plywood, which affects the overall aesthetics; ④ It is necessary to use a continuous press for multiple pressings, which is costly and complicated.

[0004] It can be seen that the existing ultra-thin fiberboard has problems such as excessive formaldehyde, high water absorption thickness expansion rate, complicated process and poor aesthetics. Summary of the invention

[0005] The purpose of the embodiments of the present application is to provide a method for preparing a hard sheet, aiming to solve the problems of excessive formaldehyde, high water absorption thickness expansion rate, complex process and poor aesthetics in existing ultra-thin fiberboards.

[0006] The embodiment of the present application is implemented as follows: a method for preparing a hard sheet material comprises:

[0007] Add a polyol, a crosslinking agent and isophorone diisocyanate in a mass ratio of (35-40):(2-10):(16-40) into a reaction container, heat to 60-70°C, stir and mix evenly, add a catalyst, heat to 75-90°C and continue to react for 1-2 hours, add 2,2-dihydroxymethylpropionic acid and 1,4-butanediol and continue to react for 2-3 hours, cool to 40-45°C, add triethylamine, deionized water and ethylene-acrylic acid copolymer in sequence and mix to obtain a water-based hot melt adhesive;

[0008] Add formaldehyde, water and a modifier to a reaction container, adjust the pH to 9.0-9.5, add melamine, add caprolactam when the temperature rises to 70-90° C., and carry out heat preservation reaction at a temperature of 90-94° C. until the water solubility multiple of the mixture is 1:(1.8-2.0), adjust the pH to 9.0-9.5 when cooling, cool to 30° C.-40° C., add a coupling agent and mix to obtain a melamine formaldehyde resin;

[0009] The glass cloth is impregnated with the aqueous hot melt adhesive, and the glass fiber non-woven fabric is impregnated with the melamine formaldehyde resin, and after drying, a glass cloth prepreg and a glass fiber non-woven fabric prepreg are obtained respectively;

[0010] The glass fiber non-woven fabric prepreg is arranged in the order of an upper layer and a lower layer of the glass cloth prepreg, and a one-step hot pressing treatment is performed to obtain a hard sheet.

[0011] Another object of an embodiment of the present application is to provide a hard sheet, which is prepared by the above-mentioned method for preparing the hard sheet.

[0012] Another object of an embodiment of the present application is to provide an ultra-thin fiberboard, which is formed by hot pressing a plywood substrate, the above-mentioned hard sheet, a printing layer impregnated paper, and a wear-resistant layer impregnated paper in order from bottom to top, and then cooled by cold pressing.

[0013] The preparation method of the hard sheet provided in the embodiment of the present application uses modified low-formaldehyde melamine formaldehyde resin and water-based hot melt adhesive as the main adhesive, glass fiber non-woven fabric and glass cloth as the substrate, the glass fiber non-woven fabric and glass cloth are impregnated with the adhesive and then dried to form a semi-cured sheet, and then pressed into a board according to a specific combination method. The obtained hard sheet has the following characteristics: ① Since glass fiber is used as the main material, the color is closer to transparent color and it will be more beautiful; ② Since glass fiber lacks a large number of hydroxyl groups on wood cellulose, it will not easily absorb water and cause excessive water absorption thickness expansion rate; ③ The mixed solution of glass fiber non-woven fabric and glass cloth has a small specific surface area, which can reduce the amount of glue used and avoid excessive formaldehyde release affecting the overall formaldehyde release of the board.

[0014] In addition, the embodiment of the present application only needs to arrange the plywood, hard sheet layer, printed layer impregnated paper and wear-resistant layer impregnated paper smoothly and then press them at one time using a conventional hot press, which saves one gluing and one pressing process; the glass fiber non-woven fabric uses modified melamine formaldehyde resin, which can obtain a semi-cured sheet with a relatively uniform expansion rate. The surface of the hard sheet formed after curing is smoother and flatter, and it is not easy to form an uneven combination with the printed layer impregnated paper; the glass cloth is impregnated with water-based hot melt adhesive, which can be heated and melted again and then cooled to solidify. At the same time, the glass cloth can be used as a balance to avoid cracking caused by different thermal expansion coefficients between different layers. The internal bonding strength of the ultra-thin fiberboard prepared by the present application can reach more than 1.2MPa, and the impregnation peeling can reach the Class II plywood standard, and the 24h water absorption thickness expansion rate is less than 5%. DETAILED DESCRIPTION

[0015] In order to make the purpose, technical solution and advantages of the present application more clear, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described here are only used to explain the present application and are not used to limit the present application.

[0016] The current technology is to stick a layer of printing paper and wear-resistant paper on the surface of the board. Both types of paper are impregnated with melamine formaldehyde resin and then dried into semi-cured sheets, and then further cured into fully cured sheets through the high temperature of a hydraulic press. Because plywood cannot be pressed directly, otherwise it is easy to produce moiré, the industry has added a layer of ultra-thin fiberboard. Therefore, ultra-thin fiberboard is a very special existence in this industry. At present, continuous presses are mainly used for paving production. When it is necessary to produce ultra-thin fiberboard with a thickness of less than 1 mm, it will be very difficult, because the fiberboard production line can only use urea-formaldehyde resin and other glues with high formaldehyde content to mix with wood fibers for paving and hot pressing, which has high investment costs. At the same time, ultra-thin fiberboards are too thin to be prepared into formaldehyde-free products using MDI glue. The thinner the surface, the more difficult it is to control the paving, brushing and pre-curing layer. However, the embodiment of the present application uses a special water-based hot melt adhesive and melamine formaldehyde resin that can be dried normally to form a semi-cured sheet, and can be pressed once to prepare an ultra-thin fiberboard with controllable thickness and formaldehyde release. The equipment only needs to use the current conventional multi-layer hot press. The process is simple and flexible. The product is light-colored and will not be combined with plywood to be unsightly. There is no need to apply another layer of glue on the plywood to increase the formaldehyde industry and increase the hot pressing process.

[0017] Specifically, the present invention provides a method for preparing a hard sheet, comprising the following steps:

[0018] Step S1: Add a polyol, a cross-linking agent and isophorone diisocyanate in a mass ratio of (35-40): (2-10): (16-40) into a reaction container, heat to 60-70°C, stir and mix evenly, then add a catalyst, heat to 75-90°C and continue to react for 1-2 hours, then add 2,2-dihydroxymethylpropionic acid and 1,4-butanediol and continue to react for 2-3 hours, cool to 40-45°C, add triethylamine, deionized water and ethylene-acrylic acid copolymer in sequence and mix to obtain a water-based hot melt adhesive.

[0019] Optionally, the polyol, cross-linking agent and isophorone diisocyanate IPDI dehydrated at 110° C.-120° C. are added into a three-necked flask equipped with a stirrer and a reflux condenser in a ratio of 35-40:2-10:16-40 by mass, the mixture is heated to 60-70° C., stirred and mixed evenly, and then an appropriate amount of dibutyltin dilaurate catalyst (the addition amount is conventionally 0.2%-0.4%) is added dropwise and the temperature is raised to 75-90° C. for reaction. After reacting for 1-2 hours, 4-7 parts of 2,2-dihydroxymethylpropionic acid and 5-7 parts of 1,4-butanediol are added respectively, and the reaction is continued for 2-3 hours, and a small amount of acetone is added as a viscosity adjustment (generally, the viscosity is adjusted to within the range of 2000-3000 MPa.s), and then the reaction solution is cooled to 40-45°C, 3-5 parts of triethylamine are added to react for 10-30 minutes, 110-130 parts of deionized water are added under high-speed stirring and dispersed for 30-60 minutes, and ethylene-acrylic acid copolymer (EAA emulsion) is added according to the mass ratio of polyurethane prepolymer (aqueous polyurethane synthesized by reaction of the aforementioned polyol and isocyanate), deionized water, and EAA emulsion of 3: (1-4): 1 to mix, and a water-based hot melt adhesive emulsion is obtained.

[0020] Wherein, the polyol is one of poly(1,4-butylene adipate), polyethylene adipate, and polytetramethylene glycol monoethylene ether.

[0021] Wherein, the crosslinking agent is one or more of polypropylene oxide ether triol, trimethylolpropane, trimethylolpropane triglycidyl ether, and trimethylolpropane trimethacrylate; more preferably, it is trimethylolpropane glycidyl ether.

[0022] The average molecular weight of the cross-linking agent is 2000, 500 or a mixture of several thereof.

[0023] It is worth noting that the selection of the types of polyols and cross-linking agents has a great influence on the performance of the prepared ultra-thin fiberboard. It is difficult to achieve the strength and melting temperature required by this application by using other conventional polyester polyols or polyether polyols, and they may even fail to pass the immersion peeling test.

[0024] In addition, the present application introduces polyoxypropylene ether triol in the water-based hot melt adhesive, and controls the overall hardness and degree of cross-linking by introducing epoxy groups. Traditional water-based hot melt adhesives are relatively soft and cannot meet the requirements for preparing ultra-thin fiberboards; secondly, the EAA resin emulsion is mixed to enable it to participate in the overall cross-linking reaction. The EAA resin has good bonding to glass fiber and can be heat-sealed and melted at a lower temperature. Therefore, it can achieve 120°C hot pressing molding in the artificial board industry, while other industries use 150°C high-temperature hot pressing. That is, after being modified by the present application, it can better adapt to the process requirements of this industry.

[0025] Step S2: adding formaldehyde, water and a modifier to a reaction container, adjusting the pH to 9.0-9.5, adding melamine, and adding caprolactam when the temperature is raised to 70-90° C., and carrying out a heat preservation reaction at a temperature of 90-94° C. until the water solubility ratio of the mixture is 1:(1.8-2.0), adjusting the pH to 9.0-9.5 when cooling, cooling to 30° C.-40° C., adding a coupling agent for mixing, and obtaining a melamine formaldehyde resin.

[0026] Optionally, add 110-130 parts of 30-40% concentration formaldehyde, 50-80 parts of water, 8-15 parts of modifier into the reactor, adjust the pH value to 9.0-9.5 with caustic soda, then add 110-130 parts of melamine, add 2-5 parts of caprolactam when the temperature rises to 70-90°C, then keep warm at 90-94°C, keep warm for about 110-150 minutes, measure the water solubility, and require the water solubility of the glue to be 1:(1.8-2.0), add caustic soda when cooling, adjust the pH to 9.0-9.5, cool to 30°C-40°C, finish the glue making, and then add 1-10 parts of coupling agent for mixing.

[0027] Among them, the modifier includes three types of brightener, toughener and release agent, mainly to improve toughness and achieve rapid continuous rapid curing and demolding, and the added mass parts are 3-10 parts, 2-10 parts, and 2-10 parts respectively. Optionally, the brightener, toughener and release agent used in the embodiment of the present application are purchased from WIZ Magic Chemicals in Italy, and the models are ALTON PLAST58, ALTON 856, and ALTON HM 1010 respectively.

[0028] Wherein, the coupling agent is one of 560 silane coupling agent or 570 coupling agent or a mixture of several thereof.

[0029] It is worth noting that the embodiments of the present application can improve the toughness and impact resistance of melamine formaldehyde resin by introducing caprolactam into the synthesis of melamine formaldehyde resin, so that the molded product exhibits better mechanical strength, and can reduce the release of formaldehyde during the resin curing process, and use corresponding modifiers, modification aids and coupling agents to improve the required performance. Conventional melamine formaldehyde resin is usually modified with dioctyl phthalate or white sugar, and caprolactam has relatively better performance and will not cause whitening when pressed.

[0030] Step S3: impregnating the glass cloth with the aqueous hot melt adhesive and impregnating the glass fiber non-woven fabric with the melamine formaldehyde resin, and drying to obtain a glass cloth prepreg and a glass fiber non-woven fabric prepreg, respectively.

[0031] In this embodiment, the glass cloth is impregnated with water-based hot melt adhesive and dried to obtain a glass cloth prepreg; the glass fiber non-woven fabric is impregnated with melamine formaldehyde resin and dried to obtain a glass fiber non-woven fabric prepreg.

[0032] The weight of the glass cloth is 100 g / m 2 , woven in a horizontal and vertical manner; the quantitative amount of the glass fiber non-woven fabric is 80g / m 2 .

[0033] Among them, a drying tunnel is used for drying, the drying tunnel temperature is 110-140°C, and the operating speed is 40-60m / min.

[0034] Among them, the glass fiber non-woven fabric impregnated with melamine formaldehyde resin is controlled to have a pre-curing degree of 5%-15% after being dried in a drying oven to avoid excessive curing affecting subsequent processes.

[0035] Step S4: The glass fiber non-woven fabric prepreg is arranged in the order of the upper layer and the glass cloth prepreg is arranged in the lower layer, and a one-step hot pressing treatment is performed to obtain a hard sheet.

[0036] Among them, in the one-step hot pressing treatment, a hot pressing machine is used for hot pressing, the hot pressing temperature is 110-130°C, the hot pressing time is 1-5min, and the hot pressing pressure is 1-5mpa.

[0037] The embodiment of the present application also provides an ultra-thin fiberboard, which is obtained by hot pressing a plywood substrate, the above-mentioned hard sheet, a printing layer impregnated paper, and a wear-resistant layer impregnated paper in order from bottom to top, and then cooling them by cold pressing.

[0038] Among them, a hot press is used for one-time hot pressing and then quickly transferred to the cold pressing zone for cooling. The hot press temperature is 180℃-210℃, the time is 15-30s, the pressure is 1-5mpa, the cold pressing zone pressure is 1-5mpa, the temperature is room temperature, and the time is 10-40s.

[0039] The present application is described in detail with specific examples as follows. The experimental methods used in the following examples are conventional methods unless otherwise specified; the materials and reagents used are all commercially available unless otherwise specified.

[0040] Example 1: Preparation of hard sheet and ultra-thin fiberboard

[0041] ①First, the synthesis of water-based hot melt adhesive

[0042] Add polyadipate-1,4-butylene glycol ester, polyoxypropylene ether triol and isophorone diisocyanate IPDI dehydrated at 110°C into a three-necked flask equipped with a stirrer and a reflux condenser in a mass ratio of 40:5:16, heat to 70°C, stir and mix evenly, then drop appropriate amount of dibutyltin dilaurate catalyst and heat to 90°C for reaction. After 2h of reaction, add 5 parts of 2,2-dihydroxymethylpropionic acid and 5 parts of 1,4-butanediol respectively, continue to react for 2h, add a small amount of acetone as viscosity adjustment, then cool the reaction liquid to 45°C, add 3 parts of triethylamine to react for 30min, add 110 parts of deionized water under high-speed stirring for dispersion for 30min, and add EAA emulsion in a mass ratio of 3:1 of polyurethane prepolymer to EAA emulsion for mixing to obtain a water-based hot melt adhesive emulsion.

[0043] ②Synthesis of melamine formaldehyde resin

[0044] First, add 110 parts of 37% formaldehyde, 80 parts of water, 3 parts of brightener, 2 parts of toughening agent and 3 parts of release agent into the reactor, adjust the pH value to 9.5 with caustic soda, then add 120 parts of melamine, add 2 parts of caprolactam when the temperature reaches 90℃, and then keep it at 90℃. Keep the reaction for about 110 minutes, measure the water solubility, and the water solubility of the glue is required to be 1:2.0. Add caustic soda when cooling, adjust the pH to 9.0, cool to 40℃, finish the glue making, and then add 2 parts of coupling agent 570 for mixing.

[0045] ③ Use water-based hot melt adhesive as water-based impregnation liquid to impregnate only glass cloth, use melamine formaldehyde resin as water-based impregnation liquid to impregnate only glass fiber non-woven fabric, and use drying oven for drying after impregnation, the drying oven temperature is 110°C, and the running speed is 60m / min.

[0046] ④ Place the impregnated semi-cured sheets in the order of glass cloth semi-cured sheets on the lower layer and glass fiber non-woven fabric on the upper layer, and use a hot press to hot press to form a hard sheet. The hot pressing temperature is 110°C, the hot pressing time is 5 minutes, and the hot pressing pressure is 3Mpa.

[0047] ⑤ Arrange the plywood substrate, hard sheet, printed layer impregnated paper and wear-resistant layer impregnated paper in order from bottom to top, use a hot press to hot press them once, then quickly transfer them to the cold press area to cool down, and then take them out. The hot press temperature is 180℃, the time is 30s, the pressure is 3Mpa, the cold press area pressure is 3Mpa, the temperature is room temperature, and the time is 20s.

[0048] Example 2: Preparation of hard sheet and ultra-thin fiberboard

[0049] ①First, the synthesis of water-based hot melt adhesive

[0050] The polytetrahydrofuran diol monoethylene glycol ether, trimethylolpropane trimethacrylate and isophorone diisocyanate IPDI dehydrated at 120°C were added to a three-necked flask equipped with a stirrer and a reflux condenser in a mass ratio of 35:4:16, heated to 70°C, stirred and mixed evenly, and then an appropriate amount of dibutyltin dilaurate catalyst was added dropwise and heated to 75°C for reaction. After reacting for 2 hours, 4 parts of 2,2-dimethylolpropionic acid and 5 parts of 1,4-butanediol were added respectively, and the reaction continued for 3 hours, and a small amount of acetone was added as a viscosity adjustment, and then the reaction liquid was cooled to 40°C, 3 parts of triethylamine were added to react for 30 minutes, 110 parts of deionized water were added under high-speed stirring for dispersion for 30 minutes, and EAA emulsion was added and mixed in a mass ratio of 3:1 between polyurethane prepolymer and EAA emulsion to obtain a water-based hot melt adhesive emulsion.

[0051] ②Synthesis of melamine formaldehyde resin

[0052] First, add 130 parts of 40% concentration formaldehyde, 80 parts of water, 3 parts of brightener, 2 parts of toughening agent and 3 parts of release agent into the reactor, adjust the pH value to 9.0 with caustic soda, then add 110 parts of melamine, add 2 parts of caprolactam when the temperature reaches 70℃, then keep warm at 90℃, keep warm for about 150 minutes, measure the water solubility, and require the water solubility of the glue to be 1:2.0, add caustic soda when cooling, adjust the pH to 9.0, cool to 40℃, finish the glue making, and then add 3 parts of coupling agent 570 for mixing.

[0053] ③ Use water-based hot melt adhesive as water-based impregnation liquid to impregnate only glass cloth, use melamine formaldehyde resin as water-based impregnation liquid to impregnate only glass fiber non-woven fabric, and use drying oven for drying after impregnation, the drying oven temperature is 140°C, and the running speed is 60m / min.

[0054] ④ Place the impregnated semi-cured sheets in the order of glass cloth semi-cured sheets on the lower layer and glass fiber non-woven fabric on the upper layer, and use a hot press to hot press to form a hard sheet. The hot pressing temperature is 130°C, the hot pressing time is 1 min, and the hot pressing pressure is 1 MPa.

[0055] ⑤ Arrange the plywood substrate, hard sheet, printed layer impregnated paper and wear-resistant layer impregnated paper in order from bottom to top, use a hot press to form them once, then quickly transfer them to the cold pressing area to cool down, and then take them out. The hot press temperature is 210℃, the time is 30s, the pressure is 5Mpa, the cold pressing area pressure is 3Mpa, the temperature is room temperature, and the time is 10s.

[0056] The hard sheet and ultra-thin fiberboard prepared in the above Examples 1-2 were subjected to performance tests, and the test standards adopted were GB / T 17657-2013 and GB / T 11718-2021; the test results were: the internal bonding strength could reach 1.42MPa, the immersion peeling reached the Class II plywood standard, no debonding, the 24h water absorption thickness expansion rate reached 3.7%, and the formaldehyde value was 0.022mg / m 3 .

[0057] In addition, under the same conditions, a conventional ultra-thin fiberboard with a thickness of 1 mm on the market was pressed with impregnated paper on a 9 mm substrate at the same time as the hard sheet prepared in the embodiment of the present application. After one week, the formaldehyde release values ​​of the two were 0.35 mg / L and 0.23 mg / L, respectively. That is, the formaldehyde release of the hard sheet prepared in the present application was significantly lower than that of the conventional ultra-thin fiberboard on the market.

[0058] The following are some modification experiments on water-based hot melt adhesives in the early development process of the hard sheet of this application, as follows:

[0059] Comparative Example 1: Preparation of water-based hot melt adhesive

[0060] Add polyethylene adipate and toluene diisocyanate TDI dehydrated at 120°C into a three-necked flask equipped with a stirrer and a reflux condenser in a mass ratio of 35:16, heat to 60°C, stir and mix evenly, then drop appropriate amount of dibutyltin dilaurate catalyst and heat to 75°C for reaction. After 1 hour of reaction, add 4.5 parts of 2,2-dihydroxymethylpropionic acid and 5.5 parts of 1,4-butanediol respectively, continue to react for 2 hours, add a small amount of acetone as viscosity adjustment, then cool the reaction liquid to 40°C, add 4.5 parts of triethylamine to react for 10 minutes, and add 110 parts of deionized water for dispersion for 30 minutes under high-speed stirring.

[0061] Experimental results: The product is prone to yellowing (TDI is not resistant to yellowing), and the TDI experimental synthesis process is difficult to control, the immersion peel strength does not meet the standard, and cracks occur when boiled in water at 63°C.

[0062] Comparative Example 2: Preparation of water-based hot melt adhesive

[0063] Add polyethylene adipate and isophorone diisocyanate IPDI dehydrated at 120°C into a three-necked flask equipped with a stirrer and a reflux condenser in a mass ratio of 35:16, heat to 60°C, stir and mix evenly, then drop appropriate amount of dibutyltin dilaurate catalyst and heat to 75°C for reaction. After 1 hour of reaction, add 4.5 parts of 2,2-dihydroxymethylpropionic acid and 5.5 parts of 1,4-butanediol respectively, continue to react for 2 hours, add a small amount of acetone as viscosity adjustment, then cool the reaction liquid to 40°C, add 4.5 parts of triethylamine to react for 10 minutes, and add 110 parts of deionized water for dispersion for 30 minutes under high-speed stirring.

[0064] Experimental results: The experiment is better controlled and yellowing is no longer likely to occur, but the immersion peel strength is still not up to standard, and cracking occurs when boiled in water at 63°C. Subsequent adjustments to the type of polyol will be studied.

[0065] Comparative Example 3: Preparation of water-based hot melt adhesive

[0066] Add poly(1,4-butylene adipate) and isophorone diisocyanate (IPDI) dehydrated at 120°C into a three-necked flask equipped with a stirrer and a reflux condenser in a mass ratio of 35:16, heat to 60°C, stir and mix evenly, then drop appropriate amount of dibutyltin dilaurate catalyst and heat to 75°C for reaction. After 1 hour of reaction, add 4.5 parts of 2,2-dihydroxymethylpropionic acid and 5.5 parts of 1,4-butanediol, continue to react for 2 hours, add a small amount of acetone as a viscosity regulator, then cool the reaction solution to 40°C, add 4.5 parts of triethylamine to react for 10 minutes, and add 110 parts of deionized water for dispersion for 30 minutes under high-speed stirring.

[0067] Experimental results: The experiment is better controlled, and yellowing is not easy to occur. The impregnation peeling meets the standard, and the internal bonding strength meets the standard. However, after impregnation with the glass fiber non-woven fabric, it was found that the water absorption thickness expansion rate was greater than 6%. The type and dosage of the chain extender will be adjusted and studied later.

[0068] Comparative Example 4: Preparation of water-based hot melt adhesive

[0069] On the basis of comparative example 3, only the type or amount of the chain extender is adjusted, specifically: the chain extender is replaced from DMPA (2,2-dihydroxymethylpropionic acid) to sodium ethylenediamine sulfonate (AAS-Na), or the amount of DMPA is halved.

[0070] Experimental results: After DMPA was replaced with sodium ethylenediaminesulfonate (AAS-Na), the water absorption thickness expansion rate was greater than 7%, which actually increased; while the amount of DMPA was halved, the experiment could not be emulsified due to the reduction of hydrophilic groups.

[0071] Comparative Example 5: Preparation of water-based hot melt adhesive

[0072] On the basis of comparative example 3, a crosslinking agent was added, specifically: poly(1,4-butylene adipate), poly(propylene oxide ether triol) and isophorone diisocyanate IPDI dehydrated at 120°C were added into a three-necked flask equipped with a stirrer and a reflux condenser in a mass ratio of 35:2:16, heated to 60°C, stirred and mixed evenly, and then an appropriate amount of dibutyltin dilaurate catalyst was added dropwise and heated to 75°C for reaction. After reacting for 1 hour, 4.5 parts of 2,2-dihydroxymethylpropionic acid and 5.5 parts of 1,4-butanediol were added respectively, and the reaction was continued for 2 hours, and a small amount of acetone was added as a viscosity adjustment, and then the reaction solution was cooled to 40°C, 4.5 parts of triethylamine were added for reaction for 10 minutes, and 110 parts of deionized water were added for dispersion for 30 minutes under high-speed stirring.

[0073] Experimental results: All performances meet the standards, but it is not easy to melt at 120°C, which is not conducive to one-step direct hot pressing processing. The subsequent addition of EAA emulsion can adjust the overall hot pressing temperature.

[0074] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.

[0075] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a hard sheet, characterized in that: include: Add a polyol, a crosslinking agent and isophorone diisocyanate in a mass ratio of (35-40):(2-10):(16-40) into a reaction container, heat to 60-70°C, stir and mix evenly, add a catalyst, heat to 75-90°C and continue to react for 1-2 hours, add 2,2-dihydroxymethylpropionic acid and 1,4-butanediol and continue to react for 2-3 hours, cool to 40-45°C, add triethylamine, deionized water and ethylene-acrylic acid copolymer in sequence and mix to obtain a water-based hot melt adhesive; Add formaldehyde, water and a modifier to a reaction container, adjust the pH to 9.0-9.5, add melamine, add caprolactam when the temperature rises to 70-90° C., and carry out heat preservation reaction at a temperature of 90-94° C. until the water solubility multiple of the mixture is 1:(1.8-2.0), adjust the pH to 9.0-9.5 when cooling, cool to 30° C.-40° C., add a coupling agent and mix to obtain a melamine formaldehyde resin; The glass cloth is impregnated with the aqueous hot melt adhesive, and the glass fiber non-woven fabric is impregnated with the melamine formaldehyde resin, and after drying, a glass cloth prepreg and a glass fiber non-woven fabric prepreg are obtained respectively; The glass fiber non-woven fabric prepreg is arranged in the order of an upper layer and a lower layer of the glass cloth prepreg, and a one-step hot pressing treatment is performed to obtain a hard sheet.

2. The method for preparing a hard sheet according to claim 1, characterized in that: The polyol is one of poly(1,4-butylene adipate), polyethylene adipate and polytetramethylene glycol monoethylene ether.

3. The method for preparing a hard sheet according to claim 1, characterized in that: The crosslinking agent is one or more of polypropylene oxide ether triol, trimethylolpropane, trimethylolpropane triglycidyl ether, and trimethylolpropane trimethacrylate.

4. The method for preparing a hard sheet according to claim 3, characterized in that: The molecular weight of the cross-linking agent is 2000, 500 or a mixture of several thereof.

5. The method for preparing a hard sheet according to claim 1, characterized in that: The modifiers include brighteners, tougheners and release agents.

6. The method for preparing a hard sheet according to claim 1, characterized in that: The glass cloth has a basis weight of 100 g / m 2 , woven in a horizontal and vertical manner; the quantitative amount of the glass fiber non-woven fabric is 80g / m 2 .

7. The method for preparing a hard sheet according to claim 1, characterized in that: The drying process is carried out in a drying tunnel with a drying tunnel temperature of 110-140°C and a running speed of 40-60m / min.

8. The method for preparing a hard sheet according to claim 1, characterized in that: In the one-step hot pressing treatment, the hot pressing temperature is 110-130° C., the hot pressing time is 1-5 min, and the hot pressing pressure is 1-5 MPa.

9. A hard sheet, characterized in that: The hard sheet is prepared by the method for preparing a hard sheet according to any one of claims 1 to 8.

10. An ultra-thin fiberboard, characterized in that: The ultra-thin fiberboard is obtained by hot pressing a plywood substrate, the hard sheet material according to claim 9, a printing layer impregnated paper and a wear-resistant layer impregnated paper in order from bottom to top, and then cooling them by cold pressing.

Citation Information

Patent Citations

  • Non-formaldehyde-release consolidated composite floor and production method thereof

    CN105599414A

  • Plywood without formaldehyde release and preparation method of plywood

    CN113815063A

  • Formaldehyde-free plywood and preparation method thereof

    CN118081913A