Biomass hard carbon negative electrode material and preparation method thereof
Through the stacking reaction of biomass coke and hydrogen production reforming catalyst and the adjustment of high-temperature crystal form, the problem of difficulty and high cost of flue gas treatment in the preparation of biomass hardcock is solved, and high-efficiency and low-carbon biomass-based hardcock materials are achieved Preparation improves the performance and production efficiency of the material.
Patent Information
- Application Number
- CN202411158129.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-01
AI Technical Summary
During the preparation process of existing biomass hardcock, the flue gas volume is large, the processing is difficult, the production cost is high, and the carbon source loss is large, resulting in an increase in carbon emissions and a high catalyst cost and low efficiency.
The reforming of biomass coke and hydrogen production reforming catalyst is used to reform hydrogen production, and combined with high-temperature crystal form adjustment, the reforming of flue gas and the recycling of carbon sources is achieved, reducing production costs and carbon emissions.
The preparation of high-performance and long-life biomass-based hard carbon negative electrode materials has been achieved, which reduces production costs, improves production efficiency, reduces carbon emissions, and improves the utilization rate of carbon sources.
Smart Images

Figure CN118877874A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sodium ion batteries and mainly relates to a biomass hard carbon negative electrode material and a preparation method thereof. Background Art
[0002] The global lithium resources are unevenly distributed and the reserves are not abundant, so they cannot meet the supply demand of the global power battery and energy storage battery market. In this context, sodium-ion batteries, which work in a similar way to lithium-ion batteries, have been favored by the global new energy market and researchers due to their advantages such as wide distribution of raw materials, relatively abundant reserves, high safety, and excellent low-temperature performance. Currently, the negative electrode materials that can be used in sodium-ion batteries are mainly divided into carbon-based materials, titanium-based materials, alloy materials, and organic materials. Among them, hard carbon materials in carbon-based materials have become the most likely choice for large-scale commercial applications among the negative electrode materials of sodium-ion batteries due to their high cost-effectiveness, strong sodium storage capacity, and cheap and easy-to-obtain raw materials.
[0003] Biomass raw materials have become the preferred raw materials for hard carbon negative electrode materials of sodium ion batteries due to their low cost, wide distribution, and controllable resources. The preparation method of biomass-based hard carbon basically adopts high-temperature carbonization method, that is, the biomass raw materials are placed in a high-temperature environment, and the macromolecular composition is spontaneously heated and cracked to generate flue gas. The residual carbon is a hard carbon material, and the yield is generally 15%-30%. At present, the flue gas generated in the preparation process of biomass-based hard carbon is mostly treated by combustion method, that is, the flue gas is burned and then discharged to the outside, and the dust in the gas is collected and treated by a dust collection device. This treatment method will lose the carbon source in the biomass pyrolysis flue gas, thereby increasing production costs and carbon emissions. Therefore, carbon source recovery and comprehensive utilization of biomass pyrolysis flue gas is an important way to reduce costs and carbon emissions of biomass-based hard carbon. The existing technology for comprehensive utilization of biomass pyrolysis flue gas is to use a catalyst to convert pyrolysis flue gas into hydrogen, but there are still shortcomings such as high catalyst cost, low hydrogen recovery rate, and easy carbon deposition. Catalyst types include: catalysts containing precious metals (high cost), iron-containing catalysts (have a deteriorating effect on batteries), catalysts containing rare earth metals (complex process), fly ash catalysts (carbon deposition occurs and catalytic performance decreases), and nickel-based catalysts (low hydrogen yield).
[0004] The high-temperature carbonization method used in the preparation of biomass-based hard carbon anode materials disclosed so far will cause most of the macromolecular components in biomass to be cracked into CO, CO2, C x H y O zThe flue gas is used as a small molecule gas and then escapes, resulting in the loss of carbon source and the inability to fully utilize it. There are still problems such as large flue gas volume, difficult flue gas treatment, high production cost, large carbon source loss, and high carbon emissions. Therefore, developing a method for reforming and utilizing biomass pyrolysis flue gas to produce hydrogen and achieve comprehensive utilization while preparing high-performance and long-life biomass-based hard carbon can reduce production costs and carbon emissions, which is conducive to promoting the large-scale application of biomass-based hard carbon for sodium ion batteries and has practical significance. Summary of the invention
[0005] In order to overcome the problems in the prior art, the present invention provides a biomass hard carbon negative electrode material and a preparation method thereof, aiming to solve the technical problems in the prior art of biomass hard carbon preparation, such as large flue gas volume, difficult treatment, high production cost, large carbon source loss, etc.
[0006] In an embodiment of the present invention, a method for preparing a biomass hard carbon negative electrode material comprises the following steps:
[0007] S1. Drying and dehydrating the biomass raw material to obtain a pretreated biomass raw material;
[0008] S2, subjecting the pretreated biomass raw material to a coking treatment under inert conditions to obtain coke and pyrolysis flue gas;
[0009] S3, reforming the pyrolysis flue gas through biomass coke and a hydrogen production reforming catalyst through a stacked reaction to produce hydrogen, and then performing gas separation to obtain a combustible gas;
[0010] S4, subjecting the coke to heat treatment to adjust the crystal form to obtain a biomass hard carbon material.
[0011] In one embodiment, the biomass raw material is one or more of reeds, coconut shells, cotton stalks, bamboo, bagasse, corn stalks, and reed bamboo.
[0012] In one embodiment, the temperature of the dehydration process is 85-110° C., and the dehydration time is 12-48 hours.
[0013] In one of the embodiments, the coking treatment temperature is 200-800°C, the heating rate is 5-20°C / min, and the coking time is 1-6h.
[0014] In one embodiment, in step S3:
[0015] The biomass coke and the hydrogen production reforming catalyst are arranged in an alternating and overlapping manner to form a stacked reaction layer of the biomass coke and the hydrogen production reforming catalyst;
[0016] The pyrolysis flue gas reacts with the stacked reaction layer at a temperature of 800-1100°C.
[0017] In one embodiment, the hydrogen production reforming catalyst is a nickel-based spinel catalyst, the thickness of the biocoke layer and the hydrogen production reforming catalyst layer in the stacked reaction layer is 10 to 50 mm, and the number of layers of the biocoke layer and the hydrogen production reforming catalyst layer in the stacked reaction layer is 1 to 6.
[0018] In one embodiment, the gas separation process includes dehydrogenation treatment and denitrification treatment in sequence.
[0019] In one embodiment, the separation temperature of the dehydrogenation process is controlled to be -200 to -240°C; and the separation temperature of the denitrification process is controlled to be -192 to -195°C.
[0020] In one of the embodiments, the heating rate of the heat treatment to adjust the crystal form is 1-10°C / min, the holding temperature is 1000-1600°C, and the holding time is 1-5h.
[0021] Based on the same inventive concept, the present invention also provides a biomass hard carbon negative electrode material obtained by the above preparation method, wherein the interlayer spacing of the biomass hard carbon negative electrode material is d 002 >0.360nm, particle size is 1~10μm.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The biomass-based hard carbon negative electrode material of the present invention is based on the principle of biomass thermal cracking coking-pyrolysis flue gas reforming hydrogen production-high temperature crystal form adjustment, realizing biomass coking transformation, pyrolysis flue gas reforming hydrogen production and carbon source recovery, deep cold separation of high-value gas and biomass-based hard carbon high temperature crystal form adjustment, using biomass coke as a protective layer of reforming hydrogen production catalyst, effectively reducing the influence of foreign matter such as tar and dust on the performance of the catalyst, and using the laminated structure to enhance the reaction intensity between biomass cracking flue gas and the catalyst, so as to obtain high-performance and long-life biomass-based hard carbon negative electrode materials while realizing biomass pyrolysis flue gas reforming hydrogen production and carbon source recovery. The present invention realizes the efficient preparation of high-value-added biomass-based hard carbon materials while reducing production costs, improving production efficiency and reducing production carbon emissions. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0025] Figure 1A biomass hard carbon negative electrode material preparation device provided in an embodiment of the present invention;
[0026] Figure 2 This is a SEM image of the biomass hard carbon negative electrode material obtained in Example 1 of the present invention;
[0027] Figure 3 This is a battery cycle retention rate diagram corresponding to the biomass hard carbon negative electrode material obtained in Example 1 of the present invention as the battery negative electrode;
[0028] Description of Figure Numbers:
[0029] 101, coke chamber; 102, coke chamber wall; 103, coke chamber entrance; 104, coke chamber vent; 105, coke chamber cooling water pipeline; 106, coke chamber air outlet; 107, coke chamber thermocouple; 201, pyrolysis flue gas pipeline; 202, pipeline insulation coil; 203, pyrolysis flue gas outlet; 204, hydrogen production chamber thermocouple; 205, hydrogen production chamber wall; 206, material distribution chute; 207, hydrogen production chamber; 208, biocoke layer; 209, hydrogen production reforming layer; 210, ceramic breathable plate; 211 , mixed component gas outlet; 301, mixed component gas pipeline; 302, dehydrogenation unit; 303, dehydrogenation gas pipeline; 304, denitrification gas pipeline; 305, denitrification unit; 306, hydrogen-rich gas pipeline; 307, gas storage chamber; 308, gas composition detection system; 309, nitrogen recycling pipeline; 401, crystal adjustment chamber; 402, carbon porcelain boat; 403, crystal adjustment chamber wall; 404, crystal adjustment chamber cooling water pipeline; 405, crystal adjustment chamber thermocouple; 406, crystal adjustment chamber material inlet. DETAILED DESCRIPTION
[0030] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0031] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0032] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0033] The preparation method of the biomass hard carbon negative electrode material of the present invention comprises the following steps:
[0034] S1. Dry the biomass raw material in a blast drying oven, and then perform a stripping treatment at a temperature of 85 to 110° C. for 12 to 48 hours to obtain a pretreated biomass raw material. The biomass raw material is selected from reeds, coconut shells, cotton stalks, bamboo, bagasse, corn stalks, reed bamboo, etc.
[0035] S2. The pretreated biomass raw material is subjected to a coking treatment under inert conditions to obtain coke and pyrolysis flue gas. During the coking process, the macromolecular composition of the biomass mainly includes cellulose, lignin and hemicellulose, all of which spontaneously undergo thermal cracking at high temperatures. Hemicellulose is a carbohydrate with the worst thermal stability among the three major components. It will start to thermally crack at 180°C, first breaking from the side chain glycosidic bonds and the main chain glycosidic bonds. During the cracking process, various gaseous products are generated through reforming, dehydration, decarbonization, decarbonylation and other reactions, and coke is formed at the same time. Cellulose is also a carbohydrate with an intermediate thermal stability among the three major components. It will start to thermally crack at 240°C and crack rapidly at 320°C. Its thermal cracking generally forms oligosaccharides first, and then thermally cracks into levoglucosan (LG). Then, various gaseous products are generated through dehydration, decarbonylation, decarboxylation and other reactions, and coke is formed at the same time. Lignin is an aromatic compound with the best thermal stability among the three major components. It will generally start to thermally crack at 250°C and crack rapidly at 400°C. Its thermal cracking is mainly the thermal cracking of the benzene ring side chain at high temperature and the formation of free radicals. The thermal cracking of the side chain will form small molecular gas products and escape. The free radicals in the system combine with each other to stop the reaction, and the benzene rings existing in large quantities in lignin are difficult to completely break at high temperatures to form coke. The typical process of cellulose cracking to generate levoglucosan (LG) and coke is shown in the following formula (1). In this process, the inert condition is preferably a nitrogen atmosphere, the nitrogen atmosphere flow rate is 1 to 10 L / min, the coking temperature is 200 to 800°C, the heating rate is 5 to 20°C / min, and the coking time is 1 to 6 hours.
[0036]
[0037] S3, the pyrolysis flue gas is reformed through a stacked reaction with biomass coke and hydrogen reforming catalyst to produce hydrogen, and then the gas is separated to obtain combustible gas. The macromolecular components of cellulose, lignin and hemicellulose in biomass will produce CO, CO2, H2O, C x H y O zSince the biomass-based pyrolysis flue gas contains fine carbon particles and small ash impurities, they will adhere to the surface when passing through the hydrogen reforming catalyst and seriously reduce the catalytic efficiency. The use of biomass coke and hydrogen reforming catalyst stacked reaction structure can realize the reforming hydrogen production and carbon source recovery of biomass-based pyrolysis flue gas. The top layer of the biomass coke and hydrogen reforming catalyst stacked reaction structure is biomass coke, which can block and adsorb the fine carbon particles and small ash impurities in the biomass-based pyrolysis flue gas, thereby effectively improving the reforming hydrogen production effect of the system. When the biomass pyrolysis flue gas passes through the biomass coke layer in the stacked reaction structure, the following reactions will occur:
[0038] C x H y O z → Small molecule + H2 + coke formula (2)
[0039] C + H2O → H2 +CO Formula (3)
[0040] C + CO2 → 2 CO Formula (4)
[0041] When the biomass pyrolysis flue gas passes through the hydrogen reforming agent layer in the stacked reaction structure, small molecules and H2O / CO2 will undergo the following reactions under the catalytic action of the hydrogen reforming catalyst:
[0042] Small molecule + H2O / CO2 → CO + H2 Formula (5)
[0043] The present invention can achieve the directional conversion of biomass pyrolysis flue gas into H2 and CO gas by designing the thickness and number of layers of the stacked reaction structure of biomass coke and hydrogen production reforming catalyst, thereby effectively improving the carbon source utilization rate and reducing carbon emissions in the preparation process of biomass-based hard carbon materials. In this process, the hydrogen production reforming catalyst uses a nickel-based spinel catalyst (NiAl2O4), the thickness of the biocoke layer and the hydrogen production reforming layer is 10 to 50 mm, the number of layers of the biocoke layer and the hydrogen production reforming layer is 1 to 6 layers, and the hydrogen production reforming hydrogen production temperature in the hydrogen production chamber is controlled to be 800 to 1100°C.
[0044] Based on the different boiling points and volatility characteristics of each component in the gas, the mixed component gas is distilled to separate different gases, with the aim of obtaining a mixed gas with a high H2 / CO concentration, while recycling the inert gas N2 for subsequent high-temperature crystal adjustment process, thereby reducing production costs. The mixed component gas first enters the dehydrogenation unit along the mixed component gas pipeline, and controls the stable dehydrogenation separation temperature, thereby separating hydrogen-rich gas and CO / N2 mixed gas, wherein the hydrogen-rich gas enters the gas storage chamber along the hydrogen-rich gas pipeline for storage, and the CO / N2 mixed gas enters the denitrification unit along the dehydrogenation gas pipeline. The denitrification unit controls a stable denitrification separation temperature, thereby separating CO gas and N2 gas, wherein the CO gas enters the gas storage chamber along the denitrification gas pipeline for storage, and the N2 gas enters the nitrogen recycling pipeline and can enter the crystal adjustment chamber. The H2 / CO mixed gas stored in the gas storage chamber is detected by the gas composition detection system to obtain the concentration of H2 and CO, which can be used for methanol synthesis or water gas use. During the preparation of biomass-based hard carbon, the dehydrogenation unit controls the separation temperature to be -200 to -240°C, and the denitrification unit controls the separation temperature to be -192 to -195°C.
[0045] S4. Adjust the crystal form of the coke by heat treatment to obtain biomass hard carbon material. In the crystal adjustment stage, combined with the principle of high-temperature cracking of carbon materials, bio-coke will still undergo a series of condensation reactions to form rings at high temperatures to achieve the preparation of biomass-based hard carbon materials. After high-temperature treatment of the biochar in the crystal adjustment system, while forming a locally graphitized amorphous structure, the crystal characteristics such as interlayer spacing, graphite domain size, and lattice defects in the biomass-based hard carbon material can be adjusted. In this process, the inert protective atmosphere is nitrogen recycled from the gas separation system, the heating rate is 1-10°C / min, the insulation temperature is 1000-1600°C, and the insulation time is 1-5h.
[0046] In order to better implement the above method, an embodiment of the present invention further provides a biomass hard carbon negative electrode material preparation device, which specifically includes a biomass coking system, a reforming hydrogen production system, a gas component separation system and a crystal adjustment system.
[0047] The biomass coking system includes a coke chamber 101, a coke chamber wall 102, a coke chamber inlet 103, a coke chamber vent 104, a coke chamber cooling water pipeline 105, a coke chamber outlet 106 and a coke chamber thermocouple 107; the coke chamber vent 104 is used to introduce inert protective gas of the whole device; the coke chamber outlet 106 is used to discharge the pyrolysis flue gas generated by the biomass during the coking process, and the coke chamber cooling water pipeline 105 can introduce cooling water for water cooling protection of the biomass coking system during the coking process. In the biomass coking system, the small molecule cracking flue gas generated by the thermal cracking of the biomass is discharged from the coke chamber outlet into the reforming hydrogen production system. The coke chamber outlet 106 is connected to the hydrogen production chamber 205 through the pyrolysis flue gas pipeline 201 and the pyrolysis flue gas outlet 203. A pipeline insulation coil 202 is arranged on the outside of the pyrolysis flue gas pipeline 201. By induction heating, the temperature inside the pyrolysis flue gas pipeline is ensured to be always higher than the boiling point of the cracking flue gas, so that the pyrolysis flue gas will not condense and flow back into the coke chamber 101. The pyrolysis flue gas outlet 203 is directly connected to the hydrogen production chamber 207. A distribution chute 206 is arranged directly below the pyrolysis flue gas outlet 203. A ceramic air permeable plate 210 is arranged in the hydrogen production chamber 207 to divide the hydrogen production chamber 207 into two spaces, upper and lower. Biocoke layers 208 and hydrogen production reforming layers 209 are alternately laid on the first air permeable plate 210. A mixed component outlet 211 is arranged at the lower end of the hydrogen production chamber. In addition, a hydrogen production chamber thermocouple 204 is arranged in the hydrogen production chamber for temperature control of the reforming hydrogen production process. The hydrogen production chamber wall is made of stainless steel to reduce heat loss in the hydrogen production chamber and maintain thermal field stability. The distribution chute 206 can rotate 360 degrees to complete rotary dumping and intermittent distribution, and realize the stacking of biocoke and hydrogen production reforming catalyst with uniform thickness. The ceramic air permeable plate 210 and the mixed component outlet 211 are used to discharge the mixed component gas of the reforming hydrogen production reaction into the gas component separation system.
[0048] The mixed component gas enters the gas component separation system through the mixed component gas pipeline 301. The biomass pyrolysis flue gas will generate a low-boiling point mixed component gas containing H2, CO, and N2 after passing through the reforming hydrogen production system. The dehydrogenation unit 302 is connected to the mixed component gas pipeline 301. The top of the dehydrogenation unit 302 is connected to a hydrogen-rich gas pipeline 306, and the side of the dehydrogenation unit is connected to a dehydrogenation gas pipeline 303. The dehydrogenation gas pipeline 303 is directly connected to the denitrification unit 305, and the side of the denitrification unit 305 is connected to a denitrification gas pipeline 304, wherein the other ends of the hydrogen-rich gas pipeline 306 and the denitrification gas pipeline 304 are connected to a gas storage chamber 307, and the gas storage chamber 307 is connected to a gas composition detection system 308. A nitrogen recycling pipeline 309 is provided at the top of the denitrification unit 305, which is connected to the crystal adjustment system.
[0049] The crystal adjustment system includes a crystal adjustment chamber 401, a carbon porcelain boat is arranged at the bottom of the crystal adjustment chamber 401, a crystal adjustment thermocouple 405 is arranged inside, a cavity surrounded by a crystal adjustment chamber wall 403 of the crystal adjustment chamber 401, a crystal adjustment chamber cooling water pipe 404 is arranged outside the crystal adjustment chamber wall 403, and a crystal adjustment chamber feed port is arranged on the side wall of the crystal adjustment chamber 401. The material of the crystal adjustment chamber wall 403 is mullite, which can effectively reduce heat loss and effectively save energy consumption. The silicon molybdenum rod is used for electrical heating, and the maximum temperature of the crystal adjustment chamber can be achieved to 1750°C. The heating process relies on the temperature measurement feedback control of the coke chamber thermocouple, wherein the thermocouple adopts platinum rhodium 30-platinum rhodium 6 thermocouple (type B), the temperature measurement range is 100-1600°C, and the temperature measurement accuracy is ±1°C. The contact interface between the feed port and the crystal adjustment chamber wall is equipped with a sealing rubber ring for sealing to prevent high temperature sample oxidation. At the same time, cooling water is also arranged at the sealing rubber ring of the material port of the crystal adjustment chamber to prevent the sealing rubber ring from melting and ensure the safety of operators.
[0050] In combination with the above device, the method for preparing the biomass hard carbon negative electrode material of the present invention is as follows:
[0051] The biomass raw material is placed in a blast drying oven, dried and dehydrated, and then used to prepare the biomass hard carbon negative electrode material.
[0052] The biomass raw material obtained after dehydration is added to the coke chamber 101 through the coke chamber inlet 103, and the protective gas is introduced at a certain flow rate through the coke chamber vent 104, and the coke chamber cooling water pipeline 105 is opened. The coke chamber 101 is heated, and the temperature is controlled by the coke chamber thermocouple 107. It is kept at a certain coking temperature for a certain time. At this temperature, the macromolecular components such as cellulose, lignin, and hemicellulose in the reed biomass are cracked to produce pyrolysis flue gas. After the coking is completed, the reed-based pyrolysis flue gas is discharged from the coke chamber outlet 106 along with the protective gas.
[0053] The rotation speed of the material distribution chute 206 is adjusted, and the hydrogen production reforming catalyst and bio-coke are added respectively. Under the rotation and pouring of the material distribution chute 206, a certain bio-coke layer 208 and a hydrogen production reforming layer 209 are obtained on the ceramic air permeable plate 210. The pipeline insulation coil 202 is turned on to ensure that the reed-based pyrolysis flue gas in the pyrolysis flue gas pipeline 201 always enters the hydrogen production chamber 207 in the form of gas through the pyrolysis flue gas outlet 203, and the temperature in the hydrogen production chamber 207 is controlled by the hydrogen production chamber thermocouple 204. The biomass-based pyrolysis flue gas reacts with the bio-coke layer 208 and the hydrogen production reforming layer 209 to generate a mixed component gas containing H2, CO, and N2. The mixed component gas passes through the ceramic air permeable plate 210 and enters the mixed component gas pipeline 301 from the mixed component gas outlet 211 for subsequent gas separation.
[0054] The mixed component gas first enters the dehydrogenation unit 302 along the mixed component gas pipeline 301, and the stable dehydrogenation separation temperature is controlled to separate hydrogen-rich gas and CO / N2 mixed gas, wherein the hydrogen-rich gas enters the gas storage chamber 307 along the hydrogen-rich gas pipeline 306 for storage, and the CO / N2 mixed gas enters the denitrification unit 305 along the dehydrogenation gas pipeline 303. The denitrification unit 305 controls a stable denitrification separation temperature, and CO gas and N2 gas are separated therefrom, wherein the CO gas enters the gas storage chamber 307 along the denitrification gas pipeline 304 for storage, and the N2 gas enters the nitrogen recycling pipeline 309 and can enter the crystal adjustment chamber 401. The H2 / CO mixed gas stored in the gas storage chamber 307 is detected by the gas component detection system 308 to obtain the concentration of H2 and CO, which can be used for methanol synthesis or water gas use.
[0055] Step five, in the crystal adjustment stage, the biochar in the coke chamber 101 and the hydrogen production chamber 207 is added into the carbon-containing porcelain boat 402 in the crystal adjustment chamber 401 through the crystal adjustment chamber material port 406, the crystal adjustment chamber cooling water 404 is opened and the nitrogen recycling pipeline 309 is opened to introduce an inert protective atmosphere, the crystal adjustment chamber 401 is temperature-controlled by the crystal adjustment chamber thermocouple 405, the temperature is raised to a certain crystal adjustment temperature at a certain heating rate and kept warm for a certain time, and then naturally cooled to room temperature to obtain the biomass-based hard carbon material from the crystal adjustment chamber material port 406.
[0056] The biomass coking-reforming hydrogen production-gas component separation-crystal adjustment device designed by the present invention is developed based on the thermodynamic theory analysis and condensation separation theory in the field of biomass hard carbon negative electrode materials, combined with the basic mechanical design. This device adopts a top-down vertical construction structure, and the individual system components are reasonably designed and indispensable, and the overall equipment is scientific, unique and feasible. The complete set of equipment of the present invention has the advantages of small footprint, high integration, easy maintenance, simple operation, and efficient production. It can be used for the stable preparation of various types of biomass-based hard carbon negative electrode materials, the reforming of biomass-based pyrolysis flue gas to produce hydrogen, and the efficient utilization of carbon sources in biomass raw materials. It can effectively solve the current problems of insufficient carbon yield, difficult flue gas treatment, and high carbon emissions in the preparation process of biomass-based hard carbon materials.
[0057] The above introduces the specific implementation methods of the present application. In order to objectively illustrate the technical effects produced by the present application, the following examples and comparative examples will be used for description.
[0058] Example 1
[0059] 1000g of reed biomass raw material obtained after dehydration treatment at 90℃ for 24h is added to the coke chamber 101 through the coke chamber inlet 103, and N2 protective gas is introduced through the coke chamber vent 104 at a flow rate of 5L / min, and the coke chamber cooling water pipeline 105 is opened. The coke chamber 101 is heated, and the temperature is controlled by the coke chamber thermocouple 107, and kept at 600℃ for 3h. At this temperature, the macromolecular components such as cellulose, lignin, and hemicellulose in the reed biomass are cracked to produce pyrolysis flue gas. After the coking is completed, the reed-based pyrolysis flue gas is discharged from the coke chamber outlet 106 along with the N2 protective gas.
[0060] The rotation speed of the material distribution chute 206 is adjusted to 1.5° / s, and the hydrogen production reforming catalyst and biocoke are added respectively. Under the rotation and pouring of the material distribution chute 206, 3 layers of biocoke layer 208 and hydrogen production reforming layer 209 with a thickness of 20 mm are obtained on the ceramic permeable plate 210. The pipeline insulation coil 202 is turned on to ensure that the reed-based pyrolysis flue gas in the pyrolysis flue gas pipeline 201 always enters the hydrogen production chamber 207 in the form of gas through the pyrolysis flue gas outlet 203, and the temperature in the hydrogen production chamber 207 is controlled to be 900°C by the hydrogen production chamber thermocouple 204. After the reed-based pyrolysis flue gas reacts with the biocoke layer 208 and the hydrogen production reforming layer 209, a mixed component gas containing at least H2, CO, and N2 is generated. After passing through the ceramic permeable plate 210, the mixed component gas enters the mixed component gas pipeline 301 through the mixed component gas outlet 211 for subsequent gas separation.
[0061] The mixed component gas first enters the dehydrogenation unit 302 along the mixed component gas pipeline 301, and the separation temperature is controlled to be -210°C. The hydrogen-rich gas and the CO / N2 mixed gas are separated, wherein the hydrogen-rich gas enters the gas storage chamber 307 along the hydrogen-rich gas pipeline 306 for storage, and the CO / N2 mixed gas enters the denitrification unit 305 along the dehydrogenation gas pipeline 303. The separation temperature in the denitrification unit 305 is controlled to be -194°C, and CO gas and N2 gas are separated, wherein the CO gas enters the gas storage chamber 307 along the denitrification gas pipeline 304 for storage, and the N2 gas enters the nitrogen recycling pipeline 309 and can enter the crystal adjustment chamber 401. The H2 / CO mixed gas stored in the gas storage chamber 307 is detected by the gas composition detection system 308, and the concentration of H2 and CO is 98.4%, which can be used for methanol synthesis or water gas.
[0062] The biochar in the coke chamber 101 and the hydrogen production chamber 207 is added to the carbon porcelain boat 402 in the crystal adjustment chamber 401 through the crystal adjustment chamber material port 406, the crystal adjustment chamber cooling water pipeline 404 and the nitrogen recycling pipeline 309 are opened to introduce an inert protective atmosphere, and the crystal adjustment chamber 401 is temperature-controlled by the crystal adjustment chamber thermocouple 405, and the temperature is increased to 1400°C at a heating rate of 5°C / min and kept for 2h, and then naturally cooled to room temperature, and the reed-based hard carbon material is obtained from the crystal adjustment chamber material port 406, and its morphology is as follows: Figure 2 As shown, it can be seen that the morphology of reed-based hard carbon is irregular.
[0063] Example 2
[0064] 1000g of reed biomass raw material obtained after dehydration treatment at 90℃ for 24h is added to the coke chamber 101 through the coke chamber inlet 103, and N2 protective gas is introduced through the coke chamber vent 104 at a flow rate of 5L / min, and the coke chamber cooling water pipeline 105 is opened. The coke chamber 101 is heated, and the temperature is controlled by the coke chamber thermocouple 107, and kept at 600℃ for 3h. At this temperature, the macromolecular components such as cellulose, lignin, and hemicellulose in the reed biomass are cracked to produce pyrolysis flue gas. After the coking is completed, the reed-based pyrolysis flue gas is discharged from the coke chamber outlet 106 along with the N2 protective gas.
[0065] The rotation speed of the material distribution chute 206 is adjusted to 1.5° / s, and the hydrogen production reforming catalyst and biocoke are added respectively. Under the rotation and pouring of the material distribution chute 206, 3 layers of biocoke layer 208 and hydrogen production reforming layer 209 with a thickness of 20 mm are obtained on the ceramic permeable plate 210. The pipeline insulation coil 202 is turned on to ensure that the reed-based pyrolysis flue gas in the pyrolysis flue gas pipeline 201 always enters the hydrogen production chamber 207 in the form of gas through the pyrolysis flue gas outlet 203, and the temperature in the hydrogen production chamber 207 is controlled to be 900°C by the hydrogen production chamber thermocouple 204. After the reed-based pyrolysis flue gas reacts with the biocoke layer 208 and the hydrogen production reforming layer 209, a mixed component gas containing at least H2, CO, and N2 is generated. After passing through the ceramic permeable plate 210, the mixed component gas enters the mixed component gas pipeline 301 through the mixed component gas outlet 211 for subsequent gas separation.
[0066] The mixed component gas first enters the dehydrogenation unit 302 along the mixed component gas pipeline 301, and the separation temperature is controlled to be -210°C. The hydrogen-rich gas and the CO / N2 mixed gas are separated, wherein the hydrogen-rich gas enters the gas storage chamber 307 along the hydrogen-rich gas pipeline 306 for storage, and the CO / N2 mixed gas enters the denitrification unit 305 along the dehydrogenation gas pipeline 303. The separation temperature in the denitrification unit 305 is controlled to be -194°C, and CO gas and N2 gas are separated, wherein the CO gas enters the gas storage chamber 307 along the denitrification gas pipeline 304 for storage, and the N2 gas enters the nitrogen recycling pipeline 309 and can enter the crystal adjustment chamber 401. The H2 / CO mixed gas stored in the gas storage chamber 307 is detected by the gas composition detection system 308, and the concentration of H2 and CO is 98.4%, which can be used for methanol synthesis or water gas.
[0067] The biochar in the coke chamber 101 and the hydrogen production chamber 207 is added into the carbon-containing porcelain boat 402 in the crystal adjustment chamber 401 through the crystal adjustment chamber material port 406, the crystal adjustment chamber cooling water pipe 404 and the nitrogen recycling pipe 309 are opened to introduce an inert protective atmosphere, the crystal adjustment chamber 401 is temperature-controlled by the crystal adjustment chamber thermocouple 405, the temperature is increased to 1200°C at a heating rate of 5°C / min and kept warm for 2h, and then naturally cooled to room temperature to obtain the reed-based hard carbon material from the crystal adjustment chamber material port 406.
[0068] Example 3
[0069] 1000g of reed biomass raw material obtained after dehydration treatment at 90℃ for 24h is added to the coke chamber 101 through the coke chamber inlet 103, and N2 protective gas is introduced through the coke chamber vent 104 at a flow rate of 5L / min, and the coke chamber cooling water pipeline 105 is opened. The coke chamber 101 is heated, and the temperature is controlled by the coke chamber thermocouple 107, and kept at 600℃ for 3h. At this temperature, the macromolecular components such as cellulose, lignin, and hemicellulose in the reed biomass are cracked to produce pyrolysis flue gas. After the coking is completed, the reed-based pyrolysis flue gas is discharged from the coke chamber outlet 106 along with the N2 protective gas.
[0070] The rotation speed of the material distribution chute 206 is adjusted to 1.5° / s, and the hydrogen production reforming catalyst and biocoke are added respectively. Under the rotation and pouring of the material distribution chute 206, 3 layers of biocoke layer 208 and hydrogen production reforming layer 209 with a thickness of 20 mm are obtained on the ceramic permeable plate 210. The pipeline insulation coil 202 is turned on to ensure that the reed-based pyrolysis flue gas in the pyrolysis flue gas pipeline 201 always enters the hydrogen production chamber 207 in the form of gas through the pyrolysis flue gas outlet 203, and the temperature in the hydrogen production chamber 207 is controlled to be 900°C by the hydrogen production chamber thermocouple 204. After the reed-based pyrolysis flue gas reacts with the biocoke layer 208 and the hydrogen production reforming layer 209, a mixed component gas containing at least H2, CO, and N2 is generated. After passing through the ceramic permeable plate 210, the mixed component gas enters the mixed component gas pipeline 301 through the mixed component gas outlet 211 for subsequent gas separation.
[0071] The mixed component gas first enters the dehydrogenation unit 302 along the mixed component gas pipeline 301, and the separation temperature is controlled to be -210°C. The hydrogen-rich gas and the CO / N2 mixed gas are separated, wherein the hydrogen-rich gas enters the gas storage chamber 307 along the hydrogen-rich gas pipeline 306 for storage, and the CO / N2 mixed gas enters the denitrification unit 305 along the dehydrogenation gas pipeline 303. The separation temperature in the denitrification unit 305 is controlled to be -194°C, and CO gas and N2 gas are separated, wherein the CO gas enters the gas storage chamber 307 along the denitrification gas pipeline 304 for storage, and the N2 gas enters the nitrogen recycling pipeline 309 and can enter the crystal adjustment chamber 401. The H2 / CO mixed gas stored in the gas storage chamber 307 is detected by the gas composition detection system 308, and the concentration of H2 and CO is 98.4%, which can be used for methanol synthesis or water gas.
[0072] The biochar in the coke chamber 101 and the hydrogen production chamber 207 is added into the carbon-containing porcelain boat 402 in the crystal adjustment chamber 401 through the crystal adjustment chamber material port 406, the crystal adjustment chamber cooling water pipe 404 and the nitrogen recycling pipe 309 are opened to introduce an inert protective atmosphere, the crystal adjustment chamber 401 is temperature-controlled by the crystal adjustment chamber thermocouple 405, the temperature is increased to 1600°C at a heating rate of 5°C / min and kept warm for 2h, and then naturally cooled to room temperature to obtain the reed-based hard carbon material from the crystal adjustment chamber material port 406.
[0073] Example 4
[0074] 1000g of cotton stalk biomass raw material obtained after dehydration treatment at 90℃ for 24h was added to the coke chamber 101 through the coke chamber inlet 103, and N2 protective gas was introduced through the coke chamber vent 104 at a flow rate of 5L / min, and the coke chamber cooling water pipeline 105 was opened. The coke chamber 101 was heated, and the temperature was controlled by the coke chamber thermocouple 107, and kept at 600℃ for 3h. At this temperature, the macromolecular components such as cellulose, lignin, and hemicellulose in the reed biomass were cracked to produce pyrolysis flue gas. After the coking was completed, the reed-based pyrolysis flue gas was discharged from the coke chamber outlet 106 along with the N2 protective gas.
[0075] The rotation speed of the material distribution chute 206 is adjusted to 1.5° / s, and the hydrogen production reforming catalyst and biocoke are added respectively. Under the rotation and pouring of the material distribution chute 206, 3 layers of biocoke layer 208 and hydrogen production reforming layer 209 with a thickness of 20 mm are obtained on the ceramic permeable plate 210. The pipeline insulation coil 202 is turned on to ensure that the reed-based pyrolysis flue gas in the pyrolysis flue gas pipeline 201 always enters the hydrogen production chamber 207 in the form of gas through the pyrolysis flue gas outlet 203, and the temperature in the hydrogen production chamber 207 is controlled to be 900°C by the hydrogen production chamber thermocouple 204. After the reed-based pyrolysis flue gas reacts with the biocoke layer 208 and the hydrogen production reforming layer 209, a mixed component gas containing at least H2, CO, and N2 is generated. After passing through the ceramic permeable plate 210, the mixed component gas enters the mixed component gas pipeline 301 through the mixed component gas outlet 211 for subsequent gas separation.
[0076] The mixed component gas first enters the dehydrogenation unit 302 along the mixed component gas pipeline 301, and the separation temperature is controlled to be -210°C. The hydrogen-rich gas and the CO / N2 mixed gas are separated, wherein the hydrogen-rich gas enters the gas storage chamber 307 along the hydrogen-rich gas pipeline 306 for storage, and the CO / N2 mixed gas enters the denitrification unit 305 along the dehydrogenation gas pipeline 303. The separation temperature in the denitrification unit 305 is controlled to be -194°C, and CO gas and N2 gas are separated, wherein the CO gas enters the gas storage chamber 307 along the denitrification gas pipeline 304 for storage, and the N2 gas enters the nitrogen recycling pipeline 309 and can enter the crystal adjustment chamber 401. The H2 / CO mixed gas stored in the gas storage chamber 307 is detected by the gas composition detection system 308, and the concentration of H2 and CO is 94.8%, which can be used for methanol synthesis or water gas.
[0077] The biochar in the coke chamber 101 and the hydrogen production chamber 207 is added into the carbon-containing porcelain boat 402 in the crystal adjustment chamber 401 through the crystal adjustment chamber material port 406, the crystal adjustment chamber cooling water pipe 404 and the nitrogen recycling pipe 309 are opened to introduce an inert protective atmosphere, the crystal adjustment chamber 401 is temperature-controlled by the crystal adjustment chamber thermocouple 405, the temperature is increased to 1400°C at a heating rate of 5°C / min and kept warm for 2h, and then naturally cooled to room temperature to obtain the reed-based hard carbon material from the crystal adjustment chamber material port 406.
[0078] Example 5
[0079] 1000g of coconut shell biomass raw material obtained after dehydration treatment at 90℃ for 24h is added to the coke chamber 101 through the coke chamber inlet 103, and N2 protective gas is introduced through the coke chamber vent 104 at a flow rate of 5L / min, and the coke chamber cooling water pipeline 105 is opened. The coke chamber 101 is heated, and the temperature is controlled by the coke chamber thermocouple 107, and kept at 600℃ for 3h. At this temperature, the macromolecular components such as cellulose, lignin, and hemicellulose in the reed biomass are cracked to produce pyrolysis flue gas. After the coking is completed, the reed-based pyrolysis flue gas is discharged from the coke chamber outlet 106 along with the N2 protective gas.
[0080] The rotation speed of the material distribution chute 206 is adjusted to 1.5° / s, and the hydrogen production reforming catalyst and bio-coke are added respectively. Under the rotation and pouring of the material distribution chute 206, 3 layers of bio-coke layer 207 and hydrogen production reforming layer 208 with a thickness of 20 mm are obtained on the ceramic air permeable plate 210. The pipeline insulation coil 202 is turned on to ensure that the reed-based pyrolysis flue gas in the pyrolysis flue gas pipeline 201 always enters the hydrogen production chamber 207 in the form of gas through the pyrolysis flue gas outlet 203, and the temperature in the hydrogen production chamber 207 is controlled to be 900°C by the hydrogen production chamber thermocouple 204. After the reed-based pyrolysis flue gas reacts with the bio-coke layer 208 and the hydrogen production reforming layer 209, a mixed component gas containing at least H2, CO, and N2 is generated. After passing through the ceramic air permeable plate 210, the mixed component gas enters the mixed component gas pipeline 301 through the mixed component gas outlet 211 for subsequent gas separation.
[0081] The mixed component gas first enters the dehydrogenation unit 302 along the mixed component gas pipeline 301, and the separation temperature is controlled to be -210°C. The hydrogen-rich gas and the CO / N2 mixed gas are separated, wherein the hydrogen-rich gas enters the gas storage chamber 307 along the hydrogen-rich gas pipeline 306 for storage, and the CO / N2 mixed gas enters the denitrification unit 305 along the dehydrogenation gas pipeline 303. The separation temperature in the denitrification unit 305 is controlled to be -194°C, and CO gas and N2 gas are separated, wherein the CO gas enters the gas storage chamber 307 along the denitrification gas pipeline 304 for storage, and the N2 gas enters the nitrogen recycling pipeline 309 and can enter the crystal adjustment chamber 401. The H2 / CO mixed gas stored in the gas storage chamber 307 is detected by the gas composition detection system 308, and the concentration of H2 and CO is 96.8%, which can be used for methanol synthesis or water gas.
[0082] The biochar in the coke chamber 101 and the hydrogen production chamber 207 is added into the carbon-containing porcelain boat 402 in the crystal adjustment chamber 401 through the crystal adjustment chamber material port 406, the crystal adjustment chamber cooling water pipe 404 and the nitrogen recycling pipe 309 are opened to introduce an inert protective atmosphere, the crystal adjustment chamber 401 is temperature-controlled by the crystal adjustment chamber thermocouple 405, the temperature is increased to 1400°C at a heating rate of 5°C / min and kept warm for 2h, and then naturally cooled to room temperature to obtain the reed-based hard carbon material from the crystal adjustment chamber material port 406.
[0083] Electrical performance test:
[0084] The hard carbon material obtained in the above embodiment was mixed and ground according to the mass ratio of 90:5:5 hard carbon negative electrode material: conductive carbon black Super-P: binder PVDF (polyvinylidene fluoride), and the mixture was dissolved in NMP (N-methylpyrrolidone) as a solvent, and then coated on aluminum foil after mixing evenly, and sliced to obtain a negative electrode sheet after baking in a vacuum drying oven at 120°C for 12 hours. In a vacuum glove box, a metal sodium sheet was used as the positive electrode, the battery separator was a Whatman GF / D glass fiber separator, and the electrolyte was 1mol / LNaPF6 (DME=100Vol%), and assembled into a CR2032 button half-cell. The assembled button battery was tested for electrochemical performance in the range of 0-2V, and the results are shown in Table 1.
[0085] Table 1 Battery performance test results
[0086]
[0087] From the above examples and battery performance tests, it can be seen that the present invention achieves efficient preparation of high value-added biomass-based hard carbon materials while reducing production costs, improving production efficiency and reducing production carbon emissions. The first charge specific capacity of the biomass-based hard carbon negative electrode material is 348.83 mA hg -1The first efficiency is 87.86%, and the cycle retention rate is 94% after 1000 cycles at 1C rate. At the same time, the concentration of H2 and CO in the mixed gas recovered from pyrolysis flue gas is 98.4%.
[0088] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the scope of protection of the present invention.
Claims
1. A method for preparing a biomass hard carbon negative electrode material, characterized in that: The preparation method comprises the following steps: S1. Drying and dehydrating the biomass raw material to obtain a pretreated biomass raw material; S2, subjecting the pretreated biomass raw material to a coking treatment under inert conditions to obtain coke and pyrolysis flue gas; S3, reforming the pyrolysis flue gas through a layered reaction with biomass coke and a hydrogen production reforming catalyst to produce hydrogen, and then performing gas separation to obtain combustible gas and nitrogen; S4, subjecting the coke to heat treatment to adjust the crystal form to obtain a biomass hard carbon material.
2. The method for preparing the biomass hard carbon negative electrode material according to claim 1, characterized in that: The biomass raw material is one or more of reeds, coconut shells, cotton stalks, bamboo, bagasse, corn stalks, and reed bamboo.
3. The method for preparing the biomass hard carbon negative electrode material according to claim 1, characterized in that: The temperature of the dehydration process is 85-110° C., and the dehydration time is 12-48 hours.
4. The method for preparing the biomass hard carbon negative electrode material according to claim 1, characterized in that: The coking treatment temperature is 200-800° C., the heating rate is 5-20° C. / min, and the coking time is 1-6 hours.
5. The method for preparing the biomass hard carbon negative electrode material according to claim 1, characterized in that: In step S3: The biomass coke and the hydrogen production reforming catalyst are arranged in an alternating and overlapping manner to form a stacked reaction layer of the biomass coke and the hydrogen production reforming catalyst; The pyrolysis flue gas reacts with the stacked reaction layer at a temperature of 800-1100°C.
6. The method for preparing the biomass hard carbon negative electrode material according to claim 5, characterized in that: The hydrogen production reforming catalyst is a nickel-based spinel catalyst, the thickness of the biocoke layer and the hydrogen production reforming catalyst layer in the stacked reaction layer is 10-50 mm, and the number of layers of the biocoke layer and the hydrogen production reforming catalyst layer in the stacked reaction layer is 1-6.
7. The method for preparing the biomass hard carbon negative electrode material according to claim 1, characterized in that: The gas separation process includes dehydrogenation treatment and denitrification treatment in sequence.
8. The method for preparing the biomass hard carbon negative electrode material according to claim 7, characterized in that: The separation temperature of the dehydrogenation process is controlled to be -200 to -240°C; the separation temperature of the denitrification process is controlled to be -192 to -195°C.
9. The method for preparing the biomass hard carbon negative electrode material according to claim 1, characterized in that: The heating rate of the heat treatment to adjust the crystal form is 1-10°C / min, the insulation temperature is 1000-1600°C, and the insulation time is 1-5h.
10. The biomass hard carbon negative electrode material obtained by the preparation method according to any one of claims 1 to 9, characterized in that: The interlayer spacing of the biomass hard carbon negative electrode material is d 002 >0.360nm, particle size is 1~10μm.