Method for preparing hydroxyl gallium oxide powder in short process

Through the direct reaction between gallium salt and deionized water under ultrasonic field, the preparation process of gallium hydroxyoxide powder is simplified, the existing problems of long processes and large reagent consumption are solved, and high efficiency, environmental protection, low cost and high purity are achieved Product production, suitable for the production of high-purity gallium oxide semiconductor materials.

CN118877928APending Publication Date: 2024-11-01ANHUI UNIVERSITY OF TECHNOLOGY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410973500.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing gallium hydroxyoxide preparation process has a long process, high reagent consumption, there is a risk of impurity pollution, and high cost. It is necessary to develop a short-process, efficient and environmentally friendly preparation method.

Method used

Under the action of ultrasonic field, gallium salt reacts directly with deionized water to prepare gallium hydroxyoxide powder in one step. The process is simplified and chemical reagents are basically used. Gallium salt dissolution, ultrasonic reaction, solid-liquid separation and drying steps are used to obtain high-purity products .

Benefits of technology

It realizes the preparation of gallium hydroxyoxide powder with short process, high efficiency and low cost, reduces the risk of impurity pollution, and has strong applicability. It is suitable for the production of high-purity gallium oxide semiconductor materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of non-ferrous metallurgy, and particularly relates to a method for preparing hydroxyl gallium oxide powder through a short process. According to the method, inorganic salt of gallium is taken as a raw material, and under the action of an ultrasonic external field, gallium salt and deionized water directly react, so that the hydroxyl gallium oxide powder material is prepared in one step. According to the technical scheme, the process is short, the efficiency is high, chemical reagents are basically not used in the production process, the risk that impurity pollution is introduced from the production process or reagent raw materials is greatly reduced, high-purity products can be obtained, and the production process has the advantages of being low in cost, environmentally friendly and the like and is suitable for industrial production. The prepared hydroxyl gallium oxide powder can be directly further used for producing a high-purity gallium oxide semiconductor material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nonferrous metal metallurgy, and in particular relates to a method for preparing gallium oxyhydroxide powder in a short process. Background Art

[0002] Gallium oxide is an important semiconductor material with excellent electrical, optical and chemical properties. It is formed by the combination of gallium and oxygen and is widely used in electronic devices, optoelectronic devices and sensors. Gallium oxide has a wide band gap, which enables it to perform well in high voltage and high temperature environments. It also has good conductivity and thermal stability, making it suitable for the manufacture of high-performance power devices. In addition, its high transparency and photoconductivity make it widely used in optoelectronics, such as LEDs and solar cells. Gallium oxide is also used in gas sensors and biosensors because of its sensitivity to environmental changes. With the development of science and technology, gallium oxide also has broad application prospects in strategic emerging industries such as 5G communications and artificial intelligence, and is expected to promote innovation and development in these fields. Therefore, the development of efficient and short-process gallium oxide material preparation technology is of great significance to scientific and technological progress and social development.

[0003] Gallium oxide is usually obtained by calcining gallium oxyhydroxide at high temperature. Therefore, preparing qualified gallium oxyhydroxide is a necessary condition and technical core for producing gallium oxide.

[0004] A Chinese patent document with publication number CN107010654B discloses a method for preparing gallium oxyhydroxide using metallic gallium as a raw material, wherein metallic gallium is first dissolved in nitric acid to obtain a gallium nitrate solution, and then an alkaline solution is further added for neutralization and precipitation, and the suspension is aged and solid-liquid separated to obtain gallium oxyhydroxide powder;

[0005] A Chinese patent document with publication number CN102976393B discloses a method for preparing gallium oxyhydroxide nanocrystals, first preparing a saturated benzene solution of gallium chloride, then diluting it with 8 times the volume of benzene, further adding methanol to form a mixed solution, reacting the obtained solution at a temperature of 160 to 200° C. for 12 to 48 hours, and finally obtaining powdered gallium oxyhydroxide nanocrystals;

[0006] A Chinese patent document with publication number CN102786078B discloses a method for preparing gallium oxyhydroxide nanocrystals, wherein a saturated benzene solution of gallium chloride is diluted with benzene, a deionized aqueous solution of hexadecyltrimethylammonium bromide having a concentration of 3 to 10 mmol / L is added dropwise to the diluted solution, and the mixed system is heated to 160 to 200° C. and reacted for 10 to 18 hours to finally obtain gallium oxyhydroxide nanocrystals;

[0007] A Chinese patent document with publication number CN115974133A discloses a high-purity β-gallium oxide nano-microsphere and a preparation method thereof, wherein metal Ga is mixed with ultrapure water and subjected to a hydrothermal reaction to obtain a gallium oxyhydroxide precipitation suspension, the solid-liquid ratio of the suspension is adjusted, and the suspension is transported to an atomizing nozzle under continuous stirring, and is atomized into droplets by an atomizing gas medium, and the droplets are spheroidized by plasma to obtain high-purity β-gallium oxide nano-microspheres;

[0008] A Chinese patent document with publication number CN111592033A discloses a method for preparing target-grade gallium oxide, wherein a gallium nitrate solution having a gallium content of 25 to 55 g / L and a free nitric acid concentration of 0.1% to 10% is used as a raw material, a surfactant is added thereto, and a precipitant is further added to perform a precipitation reaction, and the product is aged, centrifugally washed, and calcined to obtain target-grade gallium oxide;

[0009] A Chinese patent document with publication number CN118026247A discloses a method for preparing gallium oxide from a gallium-containing solution. The gallium-containing solution is subjected to resin adsorption and elution in sequence to obtain a gallium-enriched solution. A composite precipitant composed of an alkali and an acid anion salt is added to the solution to obtain a gallium-rich neutralized solution. The solution is further aged, crystallized, and calcined to finally obtain a gallium oxide product.

[0010] In summary, the existing gallium oxyhydroxide / gallium oxide preparation processes generally have problems such as long process flow and high reagent consumption, and there is still a lot of room for optimization and improvement. It is necessary to further develop a gallium oxyhydroxide preparation process with a short process flow, high efficiency and environmental friendliness. Summary of the invention

[0011] The purpose of the present invention is to overcome the problems of long process flow and high reagent consumption of the existing gallium oxyhydroxide preparation process, and provide a method for preparing gallium oxyhydroxide powder in a short process. The process technology of the present invention is short and efficient, and basically no chemical reagents are used in the production process, which not only greatly reduces the risk of impurity contamination introduced by the production process or reagent raw materials, but also is conducive to obtaining high-purity products, and the production process has the advantages of low cost and environmental friendliness, and the prepared gallium oxyhydroxide powder can be directly further used to produce high-purity gallium oxide semiconductor materials.

[0012] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0013] The invention provides a method for preparing gallium oxyhydroxide powder in a short process. Gallium salt and deionized water are directly reacted under the action of an ultrasonic external field to prepare gallium oxyhydroxide powder material in one step.

[0014] Furthermore, the method for preparing gallium oxyhydroxide powder by the short process as described above specifically comprises the following steps:

[0015] 1) dissolving a gallium salt in deionized water to obtain a gallium salt solution of a certain concentration;

[0016] 2) placing the gallium salt solution in a sealed reaction container, sealing it and turning on the ultrasonic external field to allow the gallium salt to react directly with deionized water to generate gallium oxyhydroxide;

[0017] 3) After the reaction is completed, the mixture is cooled to room temperature and solid-liquid separation is performed on the obtained mixed slurry;

[0018] 4) Drying the filter residue to obtain gallium oxyhydroxide powder material.

[0019] Furthermore, in step 1), the gallium salt is one of gallium sulfate, gallium nitrate and gallium chloride.

[0020] Furthermore, in step 1), the concentration of the gallium salt solution is 0.05-5.5 mol / L.

[0021] Furthermore, in step 2), the ultrasonic frequency is 10 to 200 kHz.

[0022] Furthermore, in step 2), the reaction temperature is 60 to 260° C., the system pressure is the natural pressure under the temperature conditions, and the reaction time is 2 to 18 hours.

[0023] Furthermore, in step 3), the filter residue produced by solid-liquid separation is washed 2 to 6 times with deionized water.

[0024] Furthermore, in step 4), the filter residue is dried at 110-160° C. for 12-72 hours.

[0025] The beneficial effects of the present invention are:

[0026] 1. A short-process method for preparing gallium oxyhydroxide powder of the present invention can obtain gallium oxyhydroxide powder material through a one-step reaction between gallium salt and water. The process is short and efficient, which can not only reduce the energy consumption and cost of the production process, but also effectively avoid the risk of introducing impurities due to the complex production process, which is conducive to obtaining high-purity products.

[0027] 2. The present invention discloses a short-process method for preparing gallium oxyhydroxide powder, which uses simple gallium salt and water as raw materials, and can obtain gallium oxyhydroxide powder material through a one-step conversion. The reaction process does not require the use of chemical reagents such as acids and alkalis, which not only effectively reduces the cost of using reagent raw materials, but also can greatly reduce the risk of introducing impurities from the reaction raw materials. In addition, the gallium salt used in the patented technology has a wide range of sources, and whether it is gallium nitrate, gallium chloride or gallium sulfate, it can achieve efficient conversion of gallium oxyhydroxide powder, and has strong adaptability to raw materials.

[0028] 3. A short-process method for preparing gallium oxyhydroxide powder of the present invention can make gallium ions fully dispersed and efficiently contact in an aqueous medium under ultrasonic external field conditions. At the same time, gallium ions and water molecules have high surface activity under the ultrasonic external field, which can make the conversion process efficient and rapid. Compared with the traditional mechanical stirring reactor, the ultrasonic external field can provide more sufficient kinetic conditions for the reaction process, improve the reaction efficiency and conversion rate, and the ultrasonic equipment is commonly used in the field of metallurgical materials. The equipment is simple and easy to operate, and the investment cost is low. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] The present invention discloses a method for preparing gallium oxyhydroxide powder in a short process, wherein an inorganic salt of gallium is used as a raw material, and the gallium salt is directly reacted with deionized water under the action of an ultrasonic external field to prepare gallium oxyhydroxide powder material in one step. The technical solution of the present invention has a short process and high efficiency, and basically no chemical reagents are used in the production process. This not only greatly reduces the risk of impurity contamination introduced by the production process or reagent raw materials, which is conducive to obtaining high-purity products, but also the production process has the advantages of low cost and environmental friendliness. The prepared gallium oxyhydroxide powder can be directly further used to produce high-purity gallium oxide semiconductor materials. The production process of the present invention specifically includes the following steps:

[0031] 1) dissolving a gallium salt (one of gallium sulfate, gallium nitrate and gallium chloride) in deionized water to obtain a gallium salt solution with a concentration of 0.05 to 5.5 mol / L;

[0032] 2) placing the gallium salt solution in a sealed reaction container, sealing it, turning on the ultrasonic external field, the ultrasonic frequency is 10 to 200 kHz, the system is heated to 60 to 260° C., reacting for 2 to 18 hours, so that the gallium salt reacts directly with deionized water to generate gallium oxyhydroxide;

[0033] 3) After the reaction is completed, the mixture is cooled to room temperature, and the obtained mixed slurry is subjected to solid-liquid separation, and the obtained filter residue is washed with deionized water for 2 to 6 times;

[0034] 4) Drying the filter residue at 110-160° C. for 12-72 hours to obtain gallium oxyhydroxide powder material.

[0035] The relevant specific embodiments of the present invention are as follows:

[0036] Example 1

[0037] A method for preparing gallium oxyhydroxide powder in a short process according to the present embodiment specifically comprises the following steps:

[0038] 1) dissolving gallium chloride in deionized water to obtain a gallium salt solution with a concentration of 5.5 mol / L;

[0039] 2) placing the gallium salt solution in a sealed reaction container, sealing it, and turning on the ultrasonic external field at a frequency of 10 kHz. The system is heated to 60° C. and reacted for 18 hours to allow the gallium salt to directly react with deionized water to generate gallium oxyhydroxide;

[0040] 3) After the reaction is completed, the mixture is cooled to room temperature, and the obtained mixed slurry is subjected to solid-liquid separation, and the obtained filter residue is washed 6 times with deionized water;

[0041] 4) Drying the filter residue at 160° C. for 12 h to obtain gallium oxyhydroxide powder material.

[0042] The obtained gallium oxyhydroxide powder was weighed and analyzed by inductively coupled plasma mass spectrometry (ICP-MS) using the treatment method of this embodiment. The results showed that the conversion rate of gallium chloride to gallium oxyhydroxide was 99.61%.

[0043] Example 2

[0044] A method for preparing gallium oxyhydroxide powder in a short process according to the present embodiment specifically comprises the following steps:

[0045] 1) dissolving gallium nitrate in deionized water to obtain a gallium salt solution with a concentration of 0.05 mol / L;

[0046] 2) placing the gallium salt solution in a sealed reaction container, sealing it, turning on the ultrasonic external field, the ultrasonic frequency is 200kHz, the system is heated to 260°C, and reacting for 2h, so that the gallium salt reacts directly with deionized water to generate gallium oxyhydroxide;

[0047] 3) After the reaction is completed, the mixture is cooled to room temperature, solid-liquid separation is performed on the obtained mixed slurry, and the obtained filter residue is washed twice with deionized water;

[0048] 4) Drying the filter residue at 110° C. for 72 h to obtain gallium oxyhydroxide powder material.

[0049] The obtained gallium oxyhydroxide powder was weighed and analyzed by inductively coupled plasma mass spectrometry (ICP-MS) using the treatment method of this embodiment. The results showed that the conversion rate of gallium nitrate to gallium oxyhydroxide was 98.86%.

[0050] Example 3

[0051] A method for preparing gallium oxyhydroxide powder in a short process according to the present embodiment specifically comprises the following steps:

[0052] 1) dissolving gallium sulfate in deionized water to obtain a gallium salt solution with a concentration of 2.0 mol / L;

[0053] 2) placing the gallium salt solution in a sealed reaction container, sealing it, and turning on the ultrasonic external field at a frequency of 50 kHz. The system is heated to 100° C. and reacted for 6 hours to allow the gallium salt to directly react with deionized water to generate gallium oxyhydroxide;

[0054] 3) After the reaction is completed, the mixture is cooled to room temperature, solid-liquid separation is performed on the obtained mixed slurry, and the obtained filter residue is washed 3 times with deionized water;

[0055] 4) Drying the filter residue at 120° C. for 60 h to obtain gallium oxyhydroxide powder material.

[0056] The obtained gallium oxyhydroxide powder was weighed and analyzed by inductively coupled plasma mass spectrometry (ICP-MS) using the treatment method of this embodiment. The results showed that the conversion rate of gallium sulfate to gallium oxyhydroxide was 99.16%.

[0057] Example 4

[0058] A method for preparing gallium oxyhydroxide powder in a short process according to the present embodiment specifically comprises the following steps:

[0059] 1) dissolving gallium sulfate in deionized water to obtain a gallium salt solution with a concentration of 3.0 mol / L;

[0060] 2) placing the gallium salt solution in a sealed reaction container, sealing it, turning on the ultrasonic external field, the ultrasonic frequency is 100 kHz, the system is heated to 150°C, and reacting for 10 hours, so that the gallium salt reacts directly with deionized water to generate gallium oxyhydroxide;

[0061] 3) After the reaction is completed, the mixture is cooled to room temperature, and the obtained mixed slurry is subjected to solid-liquid separation, and the obtained filter residue is washed 4 times with deionized water;

[0062] 4) Drying the filter residue at 130° C. for 48 h to obtain gallium oxyhydroxide powder material.

[0063] The obtained gallium oxyhydroxide powder was weighed and analyzed by inductively coupled plasma mass spectrometry (ICP-MS) using the treatment method of this embodiment. The results showed that the conversion rate of gallium sulfate to gallium oxyhydroxide was 99.67%.

[0064] Example 5

[0065] A method for preparing gallium oxyhydroxide powder in a short process according to the present embodiment specifically comprises the following steps:

[0066] 1) dissolving gallium nitrate in deionized water to obtain a gallium salt solution with a concentration of 4.5 mol / L;

[0067] 2) placing the gallium salt solution in a sealed reaction container, sealing it, turning on the ultrasonic external field, the ultrasonic frequency is 150kHz, the system is heated to 200°C, and reacting for 12 hours, so that the gallium salt reacts directly with deionized water to generate gallium oxyhydroxide;

[0068] 3) After the reaction is completed, the mixture is cooled to room temperature, and the obtained mixed slurry is subjected to solid-liquid separation, and the obtained filter residue is washed 5 times with deionized water;

[0069] 4) Drying the filter residue at 140° C. for 24 h to obtain gallium oxyhydroxide powder material.

[0070] The obtained gallium oxyhydroxide powder was weighed and analyzed by inductively coupled plasma mass spectrometry (ICP-MS) using the treatment method of this embodiment. The results showed that the conversion rate of gallium nitrate to gallium oxyhydroxide was 99.72%.

[0071] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing gallium oxyhydroxide powder by a short process, It is characterized in that Under the action of an ultrasonic external field, gallium salt and deionized water are directly reacted to prepare gallium oxyhydroxide powder material in one step.

2. The method for preparing gallium oxyhydroxide powder by a short process according to claim 1, It is characterized in that The specific steps include: 1) dissolving a gallium salt in deionized water to obtain a gallium salt solution of a certain concentration; 2) placing the gallium salt solution in a sealed reaction container, sealing it and turning on the ultrasonic external field to allow the gallium salt to react directly with deionized water to generate gallium oxyhydroxide; 3) After the reaction is completed, the mixture is cooled to room temperature and solid-liquid separation is performed on the obtained mixed slurry; 4) Drying the filter residue to obtain gallium oxyhydroxide powder material.

3. The method for preparing gallium oxyhydroxide powder by a short process according to claim 2, It is characterized in that In step 1), the gallium salt is one of gallium sulfate, gallium nitrate and gallium chloride.

4. The method for preparing gallium oxyhydroxide powder by a short process according to claim 2, It is characterized in that In step 1), the concentration of the gallium salt solution is 0.05-5.5 mol / L.

5. The method for preparing gallium oxyhydroxide powder by a short process according to claim 4, It is characterized in that In step 2), the ultrasonic frequency is 10 to 200 kHz.

6. The method for preparing gallium oxyhydroxide powder by a short process according to claim 2, It is characterized in that In step 2), the reaction temperature is 60 to 260° C., the system pressure is the natural pressure under the temperature conditions, and the reaction time is 2 to 18 hours.

7. The method for preparing gallium oxyhydroxide powder by a short process according to claim 2, It is characterized in that In step 3), the filter residue produced by solid-liquid separation is washed 2 to 6 times with deionized water.

8. The method for preparing gallium oxyhydroxide powder by a short process according to claim 2, It is characterized in that In step 4), the filter residue is dried at 110-160° C. for 12-72 hours.

Citation Information

Patent Citations

  • Preparation method of hydroxyl gallium oxide nanometer crystal

    CN102786078B

  • Preparation method of gallium oxide hydroxide nano-crystals

    CN102976393B

  • A method for preparing monodisperse gallium oxide powder and its high-density ceramic target.

    CN107010654B

  • Preparation method of target-grade gallium oxide

    CN111592033A

  • High-purity beta gallium oxide nano-microsphere and preparation method thereof

    CN115974133A