Preparation method and application of gas sensitive material Bi2MoO6
Bi2MoO6 gas-sensitive material was prepared by hydrothermal method, and its structure was adjusted using surfactant, which solved the problem of low sensitivity of existing gas-sensitive materials, achieved high sensitivity detection of ethanol gas, high response strength, high detection sensitivity, and It has rapid detection capabilities at low temperatures.
Patent Information
- Application Number
- CN202411119487.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-01
AI Technical Summary
The existing gas-sensitive materials have small response strength, low detection sensitivity, poor performance at low temperatures, and high temperature operation increases power consumption and affects the stability of the sensor.
Bi2MoO6 gas-sensitive material is prepared by hydrothermal method. By adding surfactant to the suspension, the pH value is adjusted and hydrothermal reaction is carried out in an autoclave to form Bi2MoO6 material with a unique layered structure and tiny nanosheets, which is enlarged. The specific surface area is improved and the gas-sensitive performance is improved.
It realizes high sensitivity detection of ethanol gas, has high response strength and high detection sensitivity, and can quickly detect low-concentration ethanol at low temperatures. It has a simple preparation process, high purity, good crystallinity and uniformity.
Smart Images

Figure CN118877939A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of gas sensing, and specifically, to a preparation method and application of a gas-sensitive material Bi2MoO6. Background Art
[0002] Ethanol is a volatile, colorless and transparent liquid widely used in industrial production, medical and other fields. Long-term exposure to high concentrations of ethanol can irritate the respiratory tract, nasal cavity, oral cavity and mucous membranes. In more serious cases, it can cause hepatitis and affect the brain, leading to various neurological and psychological diseases. Therefore, sensitive detection of ethanol and its concentration is required in both industrial production and life.
[0003] Common ethanol gas-sensitive materials include metal oxide semiconductors such as SnO2, ZnO, TiO2, and Fe2O3. They have poor selectivity, are easily interfered by other gases, and have high operating temperatures, and poor sensitivity at low temperatures. As a ternary metal oxide semiconductor, Bi2MoO6 has good selectivity, but gas molecules are not easily adsorbed on its surface, which makes the interaction intensity between the gas-sensitive material and the gas molecules smaller, resulting in a smaller gas-sensitive response and poorer sensitivity. Generally, the detection sensitivity is improved by increasing the operating temperature of the gas-sensitive material. However, higher temperatures will increase power consumption and affect the stability and life of the sensor.
[0004] In summary, the existing gas-sensitive materials have a small response intensity and low detection sensitivity. Summary of the invention
[0005] The purpose of the present invention is to provide a preparation method and application of a gas-sensitive material Bi2MoO6 in view of the above-mentioned deficiencies in the prior art, so as to solve the problems of low response intensity and low detection sensitivity of the gas-sensitive material in the prior art.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] The present application provides a method for preparing a gas-sensitive material Bi2MoO6, the method comprising the following steps:
[0008] Step 1, adding bismuth source powder, molybdenum source powder and surfactant into deionized water, stirring to obtain a suspension;
[0009] Step 2, adding a regulator to the suspension to adjust the pH value of the suspension to a preset pH value;
[0010] Step 3, placing the solution obtained in step 2 in a high-pressure reactor, performing a hydrothermal reaction at a preset temperature, the reaction lasts for a preset time, and naturally cooling to room temperature after the reaction is completed;
[0011] Step 4, washing, centrifuging, drying and calcining the reaction product in sequence to obtain a powdered Bi2MoO6 gas-sensitive material.
[0012] Furthermore, the bismuth source powder is Bi(NO3)3﹒5H2O, and the molybdenum source powder is Na2MoO4﹒2H2O.
[0013] Furthermore, the surfactant is one of anhydrous citric acid, L-tartaric acid, and ethylenediaminetetraacetic acid.
[0014] Furthermore, the ratio of bismuth source powder, molybdenum source powder, surfactant and deionized water is 1.669 g: 0.421 g: 0.2 mmol: 80 ml.
[0015] Furthermore, the regulator is sodium hydroxide with a concentration of 1 mol / L, and the preset pH value is 2.
[0016] Furthermore, the preset temperature is 160°C-170°C, and the preset time is 10-12h.
[0017] Furthermore, in step 4, the drying temperature is 60°C.
[0018] Furthermore, in step 4, the calcination temperature is 450° C. and the calcination time is 5 hours.
[0019] The present application also provides an application of a gas-sensitive material Bi2MoO6, where the gas-sensitive material Bi2MoO6 is used for detecting ethanol gas.
[0020] Furthermore, the gas sensitive material Bi2MoO6 is made into slurry, and the slurry is coated on a platinum electrode ceramic sheet to obtain a sensing film. After annealing, an ethanol gas sensor device is obtained, and the sensor device is placed in an environment to be detected to detect ethanol gas in the environment to be detected.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] Bi2MoO6 is a ternary metal oxide semiconductor material with a typical Aurivillius structure, consisting of [Bi2O2] 2+ The layered structure generates an internal electric field, which promotes the separation and transfer of charges. In other words, the unique interlayer structure is conducive to charge separation and transfer, thus achieving better gas sensing performance. Under the action of surfactants, the gas-sensitive material Bi2MoO6 has a mesoporous structure composed of randomly aggregated tiny nanosheets with an average pore size of about 3nm. The tiny nanosheet structure has a size of 50-300nm and a large specific surface area, reaching up to 25.430m 2 .g -1, which increases the specific surface area of the gas-sensitive material and increases the number of active sites on the surface, thereby strengthening the interaction with the ethanol gas to be detected, resulting in a greater response intensity, higher detection sensitivity, and improved gas-sensing performance.
[0023] The response value of Bi2MoO6 prepared with 0.2mmol L-tartaric acid (TA) to 100ppm ethanol at 200℃ is as high as 118, and the actual detection limit is as low as 20ppb (sensitivity is 4.13), which can realize low-temperature rapid detection of low-concentration ethanol. The gas-sensitive material of the present application has the characteristics of fast response speed, good stability, good reproducibility and high selectivity in the concentration range of 100ppm-20ppb, and the detection temperature is 100-400℃; preferably, it can be 200-250℃. In addition, the present application directly adopts the hydrothermal method for synthesis, the preparation process is simple, and the purity is high and the crystallinity and uniformity are good. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 XRD characterization results of gas-sensitive materials prepared by adding different surfactants in the preparation method of a gas-sensitive material Bi2MoO6 provided by the present invention;
[0025] Figure 2 EDS spectrum (a) of BMO-TA prepared by the preparation method of Bi2MoO6, a gas-sensitive material provided by the present invention, and the corresponding atomic percentage (b) and mass percentage (c);
[0026] Figure 3 EDS spectrum (a) of BMO-CA prepared by the preparation method of a gas-sensitive material Bi2MoO6 provided by the present invention, as well as the corresponding atomic percentage (b) and mass percentage (c);
[0027] Figure 4 EDS spectrum (a) of BMO-EDTA prepared by the preparation method of a gas-sensitive material Bi2MoO6 provided by the present invention, as well as the corresponding atomic percentage (b) and mass percentage (c);
[0028] Figure 5 EDS spectrum (a) of BMO prepared by the preparation method of a gas-sensitive material Bi2MoO6 provided by the present invention, as well as the corresponding atomic percentage (b) and mass percentage (c);
[0029] Figure 6 Image characterization of gas-sensitive materials prepared by adding different surfactants. Figure 6 (a)- Figure 6 (d) SEM images of BMO, BMO-CA, BMO-TA and BMO-EDTA respectively; Figure 6 (e) is the TEM image corresponding to BMO-CA; Figure 6 (f) is the EDS image of BMO-TA;
[0030] Figure 7 are the nitrogen adsorption-desorption isotherms and pore size distributions of BMO, BMO-CA, and BMO-TA; Figure 7 (a) is the nitrogen adsorption-desorption isotherm of BMO, Figure 7 (b) is the corresponding pore size distribution, Figure 7 (c) is the nitrogen adsorption-desorption isotherm of BMO-CA, Figure 7 (d) is the corresponding pore size distribution, Figure 7 (e) is the nitrogen adsorption-desorption isotherm of BMO-TA, Figure 7 (f) is the corresponding pore size distribution;
[0031] Figure 8 UV-visible absorption spectra of Bi2MoO6 materials prepared by adding different surfactants (a), and Tauc curve of BMO-TA (b);
[0032] Fig. 9 This is the XPS analysis result of the gas-sensitive material BMO-TA; Fig. 9 (a) Full spectrum analysis results, Fig. 9 (b) is the element Bi4f spectrum, Fig. 9 (c) is the Mo 3d spectrum, Fig. 9 (d) is the O1s spectrum;
[0033] Fig.10 The gas sensing performance test results of Bi2MoO6 materials prepared by adding different surfactants;
[0034] Fig.11 Results of long-term stability (a) and periodic testing (b) of gas-sensitive materials BMO-TA at 200°C and BMO-CA at 250°C to 100 ppm ethanol;
[0035] Fig.12 The selectivity results of BMO-TA for various volatile organic compounds at 200°C and 100 ppm are shown;
[0036] Fig.13 The gas-sensitive response of Bi2MoO6 materials prepared by adding different surfactants to different concentrations of ethanol;
[0037] Fig.14 Schematic diagram of the BMO-TA gas sensing process;
[0038] Fig.15 is the energy band diagram of the gas-sensitive material BMO-TA, Fig.15 (a) is a schematic diagram in air. Fig.15(b) is a schematic diagram in ethanol. DETAILED DESCRIPTION
[0039] In order to make the implementation process of the present invention clearer, it will be described in detail below with reference to the accompanying drawings.
[0040] Embodiment 1:
[0041] The present invention provides a method for preparing a gas-sensitive material Bi2MoO6, the method comprising the following steps:
[0042] Step 1, add bismuth source powder, molybdenum source powder, and surfactant to deionized water, stir thoroughly, and the stirring time is greater than or equal to 1h. Specifically, the bismuth source powder is Bi(NO3)3﹒5H2O (bismuth nitrate pentahydrate), the molybdenum source powder is Na2MoO4﹒2H2O (sodium molybdate dihydrate), and the surfactant is one of anhydrous citric acid (CA), L-tartaric acid (TA), and ethylenediaminetetraacetic acid (EDTA). The ratio of bismuth source powder, molybdenum source powder, surfactant, and deionized water is 1.669g:0.421g:0.2mmol:80ml, and the ratio of bismuth molybdate pentahydrate and sodium molybdate dihydrate meets the stoichiometric ratio of the reaction. 1.669g of Bi(NO3)3﹒5H2O, 0.421g of Na2MoO4﹒2H2O, and 0.2mmol of surfactant can be added to 80ml of deionized water and stirred for 1h. Surfactants can significantly reduce the surface tension of the target solution due to their molecular structure and inherent properties. Changing the type of surfactant can adjust the size and shape of Bi2MoO6.
[0043] Step 2, add a regulator to the suspension, adjust the pH value of the suspension to the preset pH value, continue stirring to make the solution fully mixed, and the stirring time is greater than or equal to 2h; the drop-by-drop method can be used, which makes it easy to control the adjustment process. The regulator is sodium hydroxide (NaOH) with a concentration of 1 mol / L, and the preset pH value is 2. The pH value will affect the structure of the prepared sample, and the pH value is 2; specifically, one of the key factors affecting the product structure is that the existence form of Bi ions when heated in a water bath depends largely on the initial pH value of the solution. When a small amount of NaOH is added to make the pH = 2, Bi(NO3)3﹒5H2O dissolves in deionized water and hydrolyzes into BiONO3 precipitate (Formula (1)). The hydrolysis product BiONO3 and MoO4 2- The ions react to form Bi2MoO6 (Formula (2)).
[0044] Bi(NO3)3+H2O→BiONO3+2H + +2NO3 - (1)
[0045] 2BiONO3+MoO4 2- →Bi2MoO6+2NO3 - (2)
[0046] Step 3, placing the solution obtained in step 2 in a high-pressure reactor. To ensure the safety of the reaction and the full progress of the hydrothermal reaction, the volume of the solution is less than or equal to four-fifths of the volume of the reactor. Carry out a hydrothermal reaction at a preset temperature, the preset temperature is 160°C-170°C, preferably, the preset temperature is 160°C; a sufficiently high temperature can allow the reactants to fully react and generate more products, but too high a temperature will cause power loss, which is not conducive to economic benefits. The reaction lasts for a preset time, the preset time is 10-12h; ensure that there is enough time for a full reaction. After the reaction is completed, cool naturally to room temperature.
[0047] Step 4, washing, centrifuging, drying and calcining the reaction product in sequence to obtain a powdered Bi2MoO6 gas-sensitive material. The product is washed and centrifuged with deionized water and anhydrous ethanol. The purpose of washing is to effectively remove impurities and unreacted raw materials, and the purpose of centrifugation is to separate the solid product from the liquid. Specifically, the washing is to alternately add deionized water and ethanol and centrifuge, and then pour out the deionized water and ethanol to remove impurities soluble in water and ethanol, thereby obtaining Bi2MoO6 of higher purity and reducing the impact on gas-sensitive reactions. Centrifugation can achieve the separation of Bi2MoO6 from the solution. Specifically, the number of washing and centrifugation is greater than or equal to 3, and the centrifugal speed is 10000rpm. Drying is drying at 60°C for 12h to fully remove moisture to prevent water molecules from occupying too many active sites, thereby affecting gas-sensitive performance. Then, high-temperature calcination at 450°C for 5h is obtained to obtain a powdered Bi2MoO6 gas-sensitive material.
[0048] The present application also provides an application of a gas-sensitive material Bi2MoO6. The gas-sensitive material Bi2MoO6 obtained by the above method can be used for detecting ethanol gas.
[0049] The gas-sensitive material Bi2MoO6 is made into a gas-sensitive layer slurry, and the slurry is coated on a platinum electrode ceramic sheet to obtain a sensing film. During coating, 3.5 ml of the slurry is taken by a pipette gun for coating; after high-temperature annealing, an ethanol gas sensor device is obtained; when in use, the sensor device is placed in a detection environment, and a four-channel detector is used for detection. The concentration of ethanol changes the resistance of the gas-sensitive material, thereby changing the change in resistance value, and calculating the gas-sensitive response value. The calculation formula of the response value is S = (R a / R g ), R a is the resistance value of the gas-sensitive material in air, R gIt is the resistance value of the gas-sensitive material in the target gas. Detection of ethanol gas in the environment to be detected is realized. Specifically, the Bi2MoO6 powder prepared by the above method is added to an agate mortar, and an appropriate amount of pine oil is taken with a plastic rubber-tipped dropper and dripped into the mortar to ensure sufficient grinding. Grind thoroughly so that the Bi2MoO6 material and pine oil are fully mixed to obtain a mixed solution. The mixed solution is evenly coated on the platinum electrode ceramic sheet. A pipette can be used. For example, a pipette with a range of 0.5ml-10ml is used to take 2.5ml of the mixed solution. The coated electrode sheet is first annealed at 70°C for 1h, and then aged at high temperature at 300°C for 12h. A hot table can be used or other heating equipment can be used. The sensing film on the surface of the electrode sheet is more solid after high-temperature aging.
[0050] Embodiment 2:
[0051] As a comparison, the difference from Example 1 is that no surfactant is added in step 1. The remaining steps are the same.
[0052] The gas-sensitive material without adding surfactant (denoted by "BMO"), the gas-sensitive material with adding anhydrous citric acid (denoted by "BMO-CA"), the gas-sensitive material with adding L-tartaric acid (denoted by "BMO-TA"), and the gas-sensitive material with adding ethylenediaminetetraacetic acid (denoted by "BMO-EDTA") were characterized and the gas-sensitive properties were tested. The results are as follows:
[0053] Figure 1 The XRD results of gas-sensitive materials prepared by adding different surfactants. From top to bottom are the spectra of BMO-EDTA, BMO-TA, BMO-CA, and BMO, and the bottom is the standard spectrum. The diffraction peaks in the XRD spectra of BMO, BMO-CA, BMO-TA, and BMO-EDTA are almost consistent with the standard peaks. The figure shows a narrow and sharp peak, and the corresponding horizontal axis is consistent with the standard peak, indicating that the gas-sensitive material prepared by the method of this application has a high degree of crystallinity. Different diffraction peaks are shown at 10.89°, 28.25°, 32.61°, 36.03°, 47.15°, 55.56°, 58.43° and 76.05° 2θ, which are consistent with the (020), (131), (002), (151), (062), (133), (262) and (193) crystal planes of JCPDS No. 72-1524. There are no peaks corresponding to impurities, and the prepared Bi2MoO6 has a high degree of crystallinity. The materials without any additives and with CA, TA and EDTA are all Bi2MoO6. Different types of surfactants have different effects on gas sensing properties. Their peak intensities and half-peak widths (FWHM) are different.
[0054] Figure 2-Figure 5EDS spectra, atomic percentages, and mass percentages of gas-sensitive materials prepared by adding different surfactants. Specifically, Figure 2 (a) is the EDS spectrum of BMO-TA, Figure 2 (b) is the atomic percentage of BMO-TA, Figure 2 (c) is the mass percentage of BMO-TA; Figure 3 (a) is the EDS spectrum of BMO-CA, Figure 3 (b) is the atomic percentage of BMO-CA, Figure 3 (c) is the mass percentage of BMO-CA; Figure 4 (a) is the EDS spectrum of BMO-EDTA, Figure 4 (b) is the atomic percentage of BMO-EDTA, Figure 4 (c) is the mass percentage of BMO-EDTA; Figure 5 (a) is the EDS spectrum of BMO, Figure 5 (b) is the atomic percentage of BMO, Figure 5 (c) is the mass percentage of BMO. According to the EDS spectrum, the elemental composition of the material can be known, and the energy spectrum shows the characteristic peaks and peak intensities of different elements in the material. Bi, Mo and O contained in the material are clearly identified. The C element in the figure is an experimental carrier element, and the tested content is higher than the actual content. According to the atomic percentage, the atomic ratio of Bi to Mo in the gas-sensitive materials BMO, BMO-CA, and BMO-EDTA is close to 2:1, while the atomic ratio of Bi to Mo in BMO-TA is equal to 2:1, which indicates that the sample is γ-Bi2MoO6 corresponding to the XRD results, rather than α and β phases.
[0055] Figure 6 Image characterization of gas-sensitive materials prepared by adding different surfactants. Figure 6 (a)- Figure 6 (d) SEM images of BMO, BMO-CA, BMO-TA and BMO-EDTA respectively; Figure 6 (e) is the TEM image corresponding to BMO-CA; Figure 6(f) is the EDS image of BMO-TA. BMO without any surfactant has an irregular large nanosheet morphology with a diameter of about 50-400nm and a certain thickness. After adding 0.2mmol CA, BMO-CA is composed of rod-shaped nanosheets with a length of about 50-300nm, and the specific surface area increases. The size of the tiny nanosheets is almost all less than 50nm, uniform and consistent, and no impurities of other shapes are found. The morphology of BMO-EDTA is similar to BMO, but after adding 0.2mmol EDTA, the large nanosheets become smaller and more irregular, and the diameter and thickness of the formed nanosheets are smaller. With the addition of 0.2mmol TA, small-sized nanosheets with uniform and smooth size are gradually formed; this shows that the addition of TA has a small size, a large specific surface area, and can provide more active sites.
[0056] Figure 7 are the nitrogen adsorption-desorption isotherms and pore size distributions of BMO, BMO-CA, and BMO-TA; Figure 7 (a) is the nitrogen adsorption-desorption isotherm of BMO, Figure 7 (b) is the corresponding pore size distribution, Figure 7 (c) is the nitrogen adsorption-desorption isotherm of BMO-CA, Figure 7 (d) is the corresponding pore size distribution, Figure 7 (e) is the nitrogen adsorption-desorption isotherm of BMO-TA, Figure 7 (f) is the corresponding pore size distribution. BET analysis will obtain specific surface area data, and nitrogen adsorption-desorption isotherms and pore size distribution diagrams can be plotted. The specific surface area and average pore size are shown in Table 1. The specific surface areas of BMO, BMO-CA and BMO-TA are 8.736, 25.430 and 17.328 m 2 .g -1 The addition of surfactants reduces the grain size and increases the specific surface area, thereby increasing the number of active sites and improving the sensitivity of ethanol detection.
[0057] Table 1: Specific surface area and average pore size of the samples
[0058]
[0059] Figure 8 The UV-visible absorption spectra of Bi2MoO6 materials prepared by adding different surfactants (a), and the Tauc curve of BMO-TA (b). It has strong light absorption ability in the wavelength range of 200-500nm, and the band gap of the prepared gas-sensitive material Bi2MoO6 is narrow. Taking BMO-TA as an example, the band gap energy (Eg) was calculated using the Kubelka-Munk function of the formula, and the Tauc curve was drawn, as shown in the figure. Figure 8As shown in (b), the band gap energy of BMO-TA is calculated to be about 2.72 eV.
[0060] Fig. 9 This is the XPS analysis result of the gas-sensitive material BMO-TA; Fig. 9 (a) Full spectrum analysis results, Fig. 9 (b) is the element Bi4f spectrum, Fig. 9 (c) is the Mo 3d spectrum, Fig. 9 (d) is the O1s spectrum. The full spectrum shows that there are three elements, Bi, Mo and O, in the material. 3+ 4f 7 / 2 and Bi 3+ 4f 5 / 2 The two peaks of BMO-TA are located at 159.31eV and 164.57eV, respectively, and the spin-orbit splitting is 5.26eV. 6+ 3d 5 / 2 and Mo 6+ 3d 3 / 2 The BMO-TA of the orbital was detected at 232.53eV and 235.67eV respectively. Gaussian theory was used to fit the XPS peak of O1s with three small peaks: lattice oxygen, surface adsorbed oxygen and hydroxyl oxygen. Fig. 9 (d) shows that two Gauss-Lorentz peaks were found at 531.59 eV and 533.35 eV of the gas-sensitive material BMO-TA, corresponding to Bi-O and Mo-O, respectively. The presence of surface adsorbed oxygen can provide active sites for the adsorption and desorption of gases, thereby improving the gas-sensing performance.
[0061] Fig.10 The gas sensing performance test results of Bi2MoO6 materials prepared by adding different surfactants. Fig.10 (a) The effect of temperature on the gas-sensitive performance of Bi2MoO6 is shown. In the temperature range of 100-400℃, the gas-sensitive responses of sensors made of different gas-sensitive materials to 100ppm ethanol at different temperatures were tested. The optimal operating temperatures of different sensors were found respectively. The gas-sensitive materials BMO and BMO-CA have the highest gas sensitivity at 250℃, which are 49.2 and 109.8 respectively. BMO-TA and BMO-EDTA have the advantage of low-temperature response, and their optimal operating temperature is 200℃, with response values of 118 and 68.2 respectively; BMO-TA has a higher response intensity at low temperatures, which is due to the fact that there are more active sites on its surface, which makes the interaction between gas and gas-sensitive materials more sufficient. Fig.10 (b) shows the curves of resistance variation of different sensors with temperature. The resistance of the sensor decreases with increasing temperature, showing a good linear relationship, demonstrating typical n-type semiconductor characteristics. Fig.10(c) shows the response-recovery curve of BMO-TA to 100 ppm ethanol at 200°C, and the response recovery situation can be obtained. Fig.10 (d) shows the response-recovery curves of BMO and BMO-CA at 250°C, BMO-TA and BMO-EDTA at 200°C to 100 ppm ethanol. The response value is calculated by the formula S = (R a / R g ) was obtained. The response of the Bi2MoO6 gas sensor with the addition of surfactant was enhanced. This is because the BMO-CA, BMO-TA, and BMO-EDTA nanosheets are small in size and have a large specific surface area, which can provide more active sites.
[0062] Fig.11 The long-term stability and periodic test results of gas-sensitive materials BMO-TA at 200°C and BMO-CA at 250°C for 100ppm ethanol are shown in Fig.11 (a) and Fig.11 (b). The sensitivity of BMO-CA varies between 90-110, with a maximum value of 109.8. The sensitivity of BMO-TA varies between 100-120, with a maximum value of 118; both have good stability.
[0063] Fig.12 The results show the selectivity of BMO-TA to various volatile organic compounds at 200℃ and 100ppm. The gas-sensitive material is sensitive to hydrogen (H2), para-xylene (C8H 10 ), isopropyl alcohol (C3H8 O ) and hydrogen sulfide (H2S) are 26.7, 15, 36 and 33 respectively, while the gas sensitive response to 100ppm ethanol is as high as 118. Obviously, the sensor's response value to ethanol is higher than that to other gases. This shows that the BMO-TA sensor has better selectivity for ethanol gas at 200℃. After adding surfactants, the specific surface area increases, the active sites become more, and it is more conducive to the adsorption of ethanol gas.
[0064] Fig.13The gas-sensitive response of Bi2MoO6 materials prepared by adding different surfactants to different concentrations of ethanol. In 100ppm ethanol, the response values of BMO-TA, BMO-CA and BMO-EDTA are 118, 109.8 and 68.2, respectively. The response value of BMO without adding any surfactant is only 49.2; surfactants can effectively improve the gas-sensitive response, and the surfactant TA has the best corresponding improvement effect. When the ethanol gas concentration is in the range of 1ppm-20ppb, the response values of BMO-CA, BMO-TA and BMO-EDTA at 1ppm ethanol concentration are 7.37, 11.2 and 8.57, respectively. The response value of BMO without adding any surfactant is only 3.92. Importantly, when the ethanol concentration is 20ppb, the response values of BMO-CA, BMO-TA and BMO-EDTA are 2.31, 4.13 and 3.32, respectively; the response value of BMO without adding any surfactant is 2.27. The larger the response value, the better the gas-sensitive performance.
[0065] Fig.14 Schematic diagram of the BMO-TA gas sensing process. When the Bi2MoO6 sensor is exposed to air at an operating temperature of 200°C, oxygen molecules in the air are adsorbed onto the sensor surface. These adsorbed oxygen molecules capture free electrons (e - ), converted to O - (Equation (3)). The adsorption of oxygen and subsequent electron capture leads to the formation of a space charge layer, also known as a depletion layer, on the surface of the Bi2MoO6 nanomaterial. This creates a potential barrier that reduces the number of free electrons in the conduction band, resulting in an increase in the sensor resistance. Upon contact with ethanol (C2H5OH) gas, ethanol molecules are adsorbed on the sensor surface (Equation (4)). The adsorbed ethanol molecules react with the surface ionic oxygen (O - ) undergoes a redox reaction. The reaction produces carbon dioxide (CO2) and water (H2O), while releasing electrons back to the conduction band of the Bi2MoO6 sensor (Equation (5)). The chemical reaction can be expressed as the release of electrons in the redox reaction reduces the height of the barrier and the thickness of the depletion layer. The increase in the conduction band electron density leads to a significant decrease in the resistance of the sensor. Therefore, the sensing mechanism relies on the reversible change in resistance caused by the interaction between the adsorbed ethanol molecules and the ionized oxygen species on the Bi2MoO6 surface.
[0066] O2(gas)+2e - → 2O - (ads) (3)
[0067] C2H5OH(gas)→C2H5OH(ads) (4)
[0068] C2H5OH(ads)+6O - (ads)→2CO2(gas)+3H2O(gas)+6e - (5)
[0069] Fig.15 is the energy band diagram of the gas-sensitive material BMO-TA, Fig.15 (a) is a schematic diagram in air. Fig.15 (b) is a schematic diagram in ethanol. The gas-sensitive material BMO-TA exhibits excellent sensing performance for low-concentration ethanol and has a low operating temperature. This is because the nanomaterial size is very small, providing a suitable pathway and abundant active sites for the transport and diffusion of ethanol molecules, thereby improving the gas-sensitive response of Bi2MoO6.
[0070] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a gas-sensitive material Bi2MoO6, characterized in that: The method comprises the following steps: Step 1, adding bismuth source powder, molybdenum source powder and surfactant into deionized water, stirring to obtain a suspension; Step 2, adding a regulator to the suspension to adjust the pH value of the suspension to a preset pH value; Step 3, placing the solution obtained in step 2 in a high-pressure reactor, performing a hydrothermal reaction at a preset temperature, the reaction lasting for a preset time, and naturally cooling to room temperature after the reaction is completed; Step 4, washing, centrifuging, drying and calcining the reaction product in sequence to obtain a powdered Bi2MoO6 gas-sensitive material.
2. The method for preparing the gas-sensitive material Bi2MoO6 according to claim 1, characterized in that: The bismuth source powder is Bi(NO3)3﹒5H2O, and the molybdenum source powder is Na2MoO4﹒2H2O.
3. The method for preparing the gas-sensitive material Bi2MoO6 according to claim 2, characterized in that: The surfactant is one of anhydrous citric acid, L-tartaric acid and ethylenediaminetetraacetic acid.
4. The method for preparing the gas-sensitive material Bi2MoO6 according to claim 3, characterized in that: The ratio of the bismuth source powder, the molybdenum source powder, the surfactant, and the deionized water is 1.669 g: 0.421 g: 0.2 mmol: 80 ml.
5. The method for preparing the gas-sensitive material Bi2MoO6 according to claim 4, characterized in that: The regulator is sodium hydroxide with a concentration of 1 mol / L, and the preset pH value is 2.
6. The method for preparing the gas-sensitive material Bi2MoO6 according to claim 5, characterized in that: The preset temperature is 160° C.-170° C., and the preset time is 10-12 hours.
7. The method for preparing the gas-sensitive material Bi2MoO6 according to claim 6, characterized in that: In step 4, the drying temperature is 60°C.
8. The method for preparing the gas-sensitive material Bi2MoO6 according to claim 7, characterized in that: In the step 4, the calcination temperature is 450° C. and the calcination time is 5 hours.
9. An application of a gas-sensitive material Bi2MoO6, characterized in that: The gas-sensitive material Bi2MoO6 is used for detecting ethanol gas.
10. The use of the gas-sensitive material Bi2MoO6 according to claim 9, characterized in that: The gas-sensitive material Bi2MoO6 is made into slurry, and the slurry is coated on a platinum electrode ceramic sheet to obtain a sensing film. After annealing, an ethanol gas sensor device is obtained, and the sensor device is placed in an environment to be detected to detect ethanol gas in the environment to be detected.