Step-by-step disintegrating slow-release oxygen composite material and preparation method thereof
By adopting a three-layer structure, the problem of unstable oxygen release rate in the prior art is solved, stable oxygen release rate and high utilization rate are achieved, and the oxidation and degradation needs of river bottom sludge are met. Environmentally friendly and non-toxic embedding agents achieve flexible oxygen release regulation.
Patent Information
- Application Number
- CN202410815491.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-06-24
AI Technical Summary
The existing sustained-release oxygen composite materials have too high oxygen release rates in the early stage and the middle and late stages have decreased, which cannot meet the needs of oxidation and degradation of river bottom sludge, and it is difficult to regulate the oxygen release rate curve, which cannot meet the needs of different water body repairs.
Using a three-layer structure, the stepwise disintegration sustained release oxygen composite material, the core layer is calcium peroxide and physically cross-linked PVA, the intermediate layer is calcium peroxide, water-soluble and water-soluble substances, and the surface layer is calcium peroxide and water-soluble The substances are gradually disintegrated by adjusting the composition and thickness of each layer and controlling the oxygen release rate.
It achieves a stable oxygen release rate, improves the utilization rate of calcium peroxide, and can flexibly regulate the oxygen release rate curve over a long period of time, meets the needs of different water body repairs, and uses environmentally friendly and non-toxic embedding agents.
Smart Images

Figure CN118878066A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of riverbed sediment treatment, and in particular to a gradually disintegrating slow-release oxygen composite material and a preparation method thereof. Background Art
[0002] Oxygenation is a common method in riverbed sediment management. Its main principle is to improve water quality by increasing the dissolved oxygen concentration in the water overlying the sediment and promoting the biochemical degradation and decomposition of various pollutants by aerobic microorganisms. There are two main methods of oxygenation: mechanical aeration and addition of oxygen-releasing agents (ORC). Mechanical aeration requires the laying of aeration equipment, which has high operating energy consumption, poor oxygenation effect on the water overlying the sediment, and inconvenient construction and operation and maintenance. Oxygen-releasing agents can be added to the sediment, and the oxygen produced can directly act on various sediments to create an aerobic environment. The oxygen bubbles produced are small and can fully contact the sediment and its overlying water during the diffusion process, maximizing the role of oxygenation in repairing water quality. Oxygen-releasing agents are easy to add and have low construction and operation costs. It is more convenient to use this method for river water restoration.
[0003] Oxygen release agents used for water body remediation are mostly peroxides, including calcium peroxide (CaO2), magnesium peroxide (MgO2), hydrogen peroxide (H2O2) and sodium percarbonate (Na2CO3·H2O2), etc., which can release oxygen and increase the dissolved oxygen value in the water when put into water and react with water. Among them, calcium peroxide has a low oxygen release rate and a long continuous release time, and has a high oxygen content and low cost, so it is the most commonly used oxygen release agent material. However, calcium peroxide is generally in powder form, and when it is put into water, it will fully contact and react with water, resulting in an excessively high initial oxygen release, which exceeds the saturated dissolved oxygen content of the water and the requirements for oxidative degradation of pollutants. The oxygen release lacks continuity, resulting in the need for multiple excessive additions, so it is necessary to use slow-release technology to control its oxygen release rate.
[0004] At present, the common method for preparing slow-release ORC is the embedding method, that is, calcium peroxide is embedded in different carriers to prepare composite ORC, and its oxygen release rate is controlled to achieve the purpose of long-term oxygen release. Commonly used embedding carriers include cement, bentonite, sodium alginate, sodium humate, polyhydroxyalkanoate (PHA), polyvinyl alcohol (PVA), etc. However, the existing embedded slow-release ORC is generally a single-layer carrier embedded oxygen release agent, and the oxygen release rate is controlled by adjusting the embedding amount. In order to ensure long-term oxygen release, a relatively small oxygen release rate is generally controlled. Therefore, in the initial period of time after being put into use, the oxygen release amount is low, and the dissolved oxygen value in the water body increases too slowly, which cannot meet the needs of oxidative degradation in the sediment. Summary of the invention
[0005] In order to solve the above problems existing in the prior art, the purpose of the present invention is to provide a gradually disintegrating slow-release oxygen composite material and a preparation method thereof, so as to overcome the above shortcomings and deficiencies existing in the prior art.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] A gradually disintegrating slow-release oxygen composite material comprises a three-layer structure of an inner core layer, an intermediate layer and a surface layer from the inside to the outside, wherein the inner core layer is made of calcium peroxide and physically cross-linked PVA; the intermediate layer is made of calcium peroxide, a water-soluble substance and a water-insoluble substance; and the surface layer is made of calcium peroxide and a water-soluble substance.
[0008] Optionally, the core material contains 30-80 wt% calcium peroxide, and / or 20-70 wt% polyvinyl alcohol, and the alcoholysis degree of the polyvinyl alcohol is above 99%.
[0009] Optionally, the water-insoluble substance in the middle layer is physically cross-linked PVA, and the water-soluble substance in the middle layer includes a water-soluble binder and a thickener, wherein the water-soluble binder is polyethylene glycol, and the thickener is xanthan gum or sodium alginate.
[0010] Optionally, the material of the intermediate layer includes the following components:
[0011]
[0012] Optionally, the water-soluble substance of the surface layer includes a water-soluble binder and a thickener, wherein the water-soluble binder is polyethylene glycol, and the thickener is xanthan gum or sodium alginate.
[0013] Optionally, the material of the surface layer includes the following components:
[0014] Calcium peroxide 40-80%;
[0015] Polyethylene glycol 20-60wt%;
[0016] Xanthan gum or sodium alginate 0-1wt%.
[0017] Optionally, the gradually disintegrating slow-release oxygen composite material is in the form of a column with a diameter of 5-25 mm and a length of 10-20 mm, preferably with a diameter of 10-12 mm; wherein the thickness of the inner core layer is 2-8 mm, the thickness of the middle layer is 5-10 mm, and the thickness of the surface layer is 2-10 mm, preferably the thickness of the inner core layer is 3-5 mm, the thickness of the middle layer is 5-6 mm, and the thickness of the surface layer is 2-5 mm.
[0018] The present invention also provides a method for preparing a gradually disintegrating slow-release oxygen composite material, comprising the following steps:
[0019] Preparation of inner core layer material: PVA particles are dissolved in deionized water under stirring at 80-95° C., the mass concentration of the PVA aqueous solution is 5-20%, the completely dissolved PVA solution is cooled to room temperature, and then cooled to 0-10° C. under refrigeration conditions, which is recorded as embedding solution 1; calcium peroxide is added to the embedding solution 1, and mechanically stirred and mixed evenly, the stirring time is 5-20 minutes, and the stirring speed is 100-300 rpm, to obtain a flowable paste, which is recorded as mixture 1, and the mixture 1 is extruded by a single screw extruder to obtain the inner core layer material;
[0020] Preparation of the intermediate layer material: PVA particles are dissolved in deionized water under stirring conditions at 80-95° C., and the mass concentration of the PVA aqueous solution is 2-10%; polyethylene glycol, xanthan gum or sodium alginate are dissolved in deionized water under stirring and mixing at room temperature to form a mixed solution, and the mixed solution is stirred and mixed with the PVA solution at room temperature in a certain proportion, which is recorded as embedding solution 2; calcium peroxide is added to the embedding solution 2, and stirred and mixed evenly, the stirring time is 5-20 minutes, and the stirring speed is 100-300rpm, to obtain a flowable paste, which is recorded as mixture 2, and the mixture 2 is extruded by a single screw extruder to prepare the intermediate layer material;
[0021] Preparation of surface material: polyethylene glycol, xanthan gum or sodium alginate are stirred and mixed at room temperature to dissolve in deionized water to obtain a mixed solution, which is recorded as embedding solution 3; calcium peroxide is added to the embedding solution 3, and stirred and mixed evenly for 5-20 minutes at a stirring speed of 100-300 rpm to obtain a flowable paste, which is recorded as mixture 3; a single-screw extruder is used to extrude mixture 3 to prepare the surface material;
[0022] Material compounding: the materials of the inner core layer, the middle layer and the surface layer are compounded in a single-hole die, and extruded to obtain a three-layer extruded material strip with a diameter of 5-25 mm. The middle layer is wrapped in the inner core layer, and the surface layer is wrapped in the middle layer. The center of the material strip is mixture 1, the middle layer is mixture 2, and the surface layer is mixture 3. The composite extrudate is cut at the extruder head to obtain a column with a length of 10-20 mm, which is then immediately frozen at -20°C for 8-12 hours, then thawed for 4 hours, and then frozen again. This is repeated 2-4 times to obtain the final product.
[0023] Optionally, in the preparation of the inner core material, the PVA concentration is preferably 8-10 wt %, and / or
[0024] The completely dissolved PVA solution is preferably cooled to 5°C under refrigeration, and / or
[0025] The mass ratio of calcium peroxide to embedding solution 1 is 1:1-1:3.
[0026] Optionally, in the preparation of the intermediate layer material, the concentration of polyethylene glycol in the mixed solution is 2-15wt%, the concentration of xanthan gum or sodium alginate is 0-2wt%, wherein the concentration of polyethylene glycol solution is preferably 5-10wt%, the concentration of xanthan gum or sodium alginate is preferably 0-0.5wt%, and / or
[0027] The mixing mass ratio of the mixed solution to the PVA solution is 1:1-1:5; and / or
[0028] The mass ratio of calcium peroxide to embedding solution 2 is 1:1-1:3.
[0029] Optionally, in the preparation of the surface material, the concentration of polyethylene glycol in the mixed solution is 5-20wt%, and the concentration of xanthan gum or sodium alginate is 0-2wt%, wherein the concentration of polyethylene glycol solution is preferably 5-10wt%, and the concentration of xanthan gum or sodium alginate is preferably 0-0.5wt%; and / or
[0030] The mass ratio of calcium peroxide to embedding solution 3 is 1:1-1:3.
[0031] Due to the adoption of the above technical solution, the present invention has the following beneficial effects:
[0032] 1. It has the characteristics of gradual disintegration, can maintain a stable oxygen release rate for a long time, and has a high utilization rate of calcium peroxide. After the traditional calcium peroxide slow-release oxygen material is put into the water body, the initial oxygen release rate is high, but the oxygen release rate will drop significantly in the middle and late stages. This is because the calcium hydroxide microcrystals formed by the reaction of calcium peroxide on the surface of the material with water will cover and block the water infiltration path, and the probability of the inner layer of calcium peroxide contacting water will be reduced, resulting in a significant decrease in its oxygen release rate, which cannot fully meet the oxygen consumption needs of microorganisms such as riverbed mud. In more serious cases, the inner layer of calcium peroxide will never react with water, resulting in a low utilization rate of calcium peroxide. The oxygen-releasing composite particles of this product have a multi-layer gradient structure inside. The surface embedding agent is a water-soluble substance, that is, a mixture of PEG and one of sodium alginate or xanthan gum. It will gradually dissolve in water and cause the surface layer to disintegrate, so that the calcium hydroxide microcrystal shell formed by the surface calcium peroxide reaction is broken, and rapid oxygen release can be achieved in the initial stage, quickly increasing the DO in the overlying water body to the saturation level, and facilitating water to penetrate into the inner layer; the middle layer embedding agent is a mixture of water-soluble and water-insoluble substances, such as a mixture of physically cross-linked PVA gel and PEG, sodium alginate or xanthan gum. When water-soluble substances such as PEG, sodium alginate or xanthan gum are dissolved, holes will be formed in the middle layer, which is convenient for water to penetrate and can maintain a medium oxygen release rate; the inner core layer embedding agent is a water-insoluble substance, such as physically cross-linked PVA gel. The PVA gel layer still has certain oxygen and water permeability, and the oxygen release rate is relatively low, which can achieve long-term oxygen release. At the same time, the particle size of the inner core layer is small, and calcium peroxide can ensure that it will eventually react completely with water, with high utilization rate.
[0033] 2. The oxygen release rate curve can be adjusted over a long period of time, with a high degree of controllable freedom, and the oxygen release cycle and oxygen release rate can be flexibly adjusted according to actual needs. The existing slow-release oxygen materials are generally a homogeneous system, that is, the oxygen release agent and the embedding agent are evenly mixed. Generally, the oxygen release rate is relatively fixed. Depending on the nature of the embedding agent, the oxygen release rate is often too fast or too slow, and it is impossible to achieve free regulation of the oxygen release rate during the long-term oxygen release process. If the embedding agent is a hydrophobic substance, the water infiltration is relatively slow, the oxygen release rate is low, and rapid oxygenation cannot be achieved in the initial stage of release, and the oxygen consumption needs of water microorganisms cannot be met; if the embedding agent is a hydrophilic substance, such as..., the oxygen release rate is relatively high, and the DO in the overlying water body increases too fast in the initial stage of release, exceeding the saturated dissolved oxygen of the water, resulting in a waste of released oxygen and shortening the oxygen release cycle. This product has a three-layer structure, which can generally achieve rapid oxygenation in the initial stage, maintain a relatively moderate oxygen release rate in the middle stage, and maintain a lower oxygen release rate in the later stage. The oxygen release rate can be freely regulated by adjusting the composition of the embedding agent in each layer and the thickness of each layer, thereby meeting the actual needs of ecological restoration of different water bodies.
[0034] 3. The embedding agent is environmentally friendly and non-toxic. The embedding agents used in this product are all environmentally friendly and non-toxic synthetic polymers or natural polymers, and no other toxic auxiliary ingredients are added during the preparation of oxygen-releasing materials. The solvent for the dissolution of water-soluble PEG, xanthan gum, and sodium alginate is water, and the PVA cross-linking adopts a physical cross-linking method of freeze-thaw cycles, avoiding the use of toxic cross-linking agents. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is the oxygen release curve diagram of the oxygen release agent of Examples 1-5 of the present invention and the comparative example. DETAILED DESCRIPTION
[0036] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0037] Embodiment 1:
[0038] PVA (polyvinyl alcohol) particles were dissolved in deionized water at 80-95° C. under stirring conditions to prepare a PVA solution with a concentration of 10 wt %, which was then cooled to room temperature and mixed with calcium peroxide at a mass ratio of 1:1 to obtain a mixture 1.
[0039] The PVA particles are dissolved in deionized water under stirring conditions at 80-95°C to prepare a PVA solution with a concentration of 5wt%, and the solution is cooled to room temperature. Then, PEG and xanthan gum are stirred, mixed and dissolved in deionized water at room temperature. The PEG concentration in the solution is 5wt%, and the xanthan gum concentration is 0.05%. The solution and the 5wt% PVA solution are stirred and mixed at a mass ratio of 1:1, and the obtained mixed solution is mixed with calcium peroxide at a mass ratio of 1:1 to obtain a mixture 2.
[0040] PEG and xanthan gum were stirred and mixed and dissolved in deionized water at room temperature, wherein the concentration of PEG (polyethylene glycol) in the solution was 10 wt % and the concentration of xanthan gum was 0.1%, and then the mixture was uniformly mixed with calcium peroxide at a mass ratio of 1:1 to obtain a mixture 3.
[0041] In a three-layer co-extrusion unit containing three single-screw extruders, mixtures 1, 2, and 3 are extruded separately, and compounded in a single-hole die. Extrusion molding obtains a three-layer extruded material strip with a diameter of 20 mm, with mixture 1 in the center and a thickness of 6 mm, mixture 2 in the middle and a thickness of 8 mm, and mixture 3 in the surface and a thickness of 6 mm. The extruded material strip is cut into a column with a length of 10 mm at the exit of the die, and then immediately frozen at -20°C for 8 hours, then thawed for 4 hours, and then frozen again. After repeating this process 3 times, the final product is obtained.
[0042] Embodiment 2:
[0043] The PVA particles were dissolved in deionized water at 80-95° C. with stirring to prepare a 10 wt % PVA solution (embedding solution 1), cooled to room temperature, and then mixed with calcium peroxide at a mass ratio of 1:1 to obtain a mixture 1.
[0044] PVA particles are dissolved in deionized water at 80-95°C with stirring to prepare a 2wt% PVA solution, which is then cooled to room temperature. PEG and xanthan gum are then stirred and mixed and dissolved in deionized water at room temperature. The PEG concentration in the solution is 10wt%, and the xanthan gum concentration is 0.05%. The solution is stirred and mixed with the 2wt% PVA solution in a mass ratio of 1:2. The resulting mixed solution is mixed with calcium peroxide in a mass ratio of 1:1 to obtain a mixture 2.
[0045] PEG and xanthan gum were stirred and mixed and dissolved in deionized water at room temperature, wherein the concentration of PEG in the solution was 10 wt % and the concentration of xanthan gum was 0.1%, and then the mixture was uniformly mixed with calcium peroxide at a mass ratio of 1:1 to obtain a mixture 3.
[0046] In a three-layer co-extrusion unit containing three single-screw extruders, mixtures 1, 2, and 3 are extruded separately, and compounded in a single-hole die. Extrusion molding is performed to obtain a three-layer extruded material strip with a diameter of 20 mm, with mixture 1 in the center and a thickness of 6 mm, mixture 2 in the middle and a thickness of 8 mm, and mixture 3 in the surface and a thickness of 6 mm. The extruded material strip is cut into a column with a length of 10 mm at the exit of the die, and then immediately frozen at -20°C for 8 hours, then thawed for 4 hours, and then frozen again. After repeating this process 3 times, the final product is obtained.
[0047] Embodiment 3:
[0048] The PVA particles were dissolved in deionized water at 80-95° C. with stirring to prepare a 10 wt % PVA solution (embedding solution 1), cooled to room temperature, and then mixed with calcium peroxide at a mass ratio of 1:1 to obtain a mixture 1.
[0049] The PVA particles were dissolved in deionized water at 80-95°C with stirring to prepare a 2wt% PVA solution, which was cooled to room temperature. PEG was then dissolved in deionized water at room temperature with stirring. The PEG concentration in the solution was 10wt%. The solution was evenly stirred and mixed with the 2wt% PVA solution at a mass ratio of 1:3. The obtained mixed solution was evenly mixed with calcium peroxide at a mass ratio of 1:1 to obtain a mixture 2.
[0050] PEG and sodium alginate were stirred and mixed and dissolved in deionized water at room temperature, wherein the concentration of PEG in the solution was 10 wt % and the concentration of sodium alginate was 0.1%, and then mixed evenly with calcium peroxide at a mass ratio of 1:1 to obtain a mixture 3.
[0051] In a three-layer co-extrusion unit containing three single-screw extruders, mixtures 1, 2, and 3 are extruded separately, and compounded in a single-hole die. Extrusion molding is performed to obtain a three-layer extruded material strip with a diameter of 20 mm, with mixture 1 in the center and a thickness of 6 mm, mixture 2 in the middle and a thickness of 8 mm, and mixture 3 in the surface and a thickness of 6 mm. The extruded material strip is cut into a column with a length of 10 mm at the exit of the die, and then immediately frozen at -20°C for 8 hours, then thawed for 4 hours, and then frozen again. After repeating this process 3 times, the final product is obtained.
[0052] Embodiment 4:
[0053] The PVA particles were dissolved in deionized water at 80-95° C. with stirring to prepare a 10 wt % PVA solution (embedding solution 1), cooled to room temperature, and then mixed with calcium peroxide at a mass ratio of 1:1 to obtain a mixture 1.
[0054] PVA particles are dissolved in deionized water at 80-95°C with stirring to prepare a 2wt% PVA solution, which is then cooled to room temperature. PEG and xanthan gum are then stirred and mixed and dissolved in deionized water at room temperature. The PEG concentration in the solution is 10wt%, and the xanthan gum concentration is 0.05%. The solution is stirred and mixed with the 2wt% PVA solution in a mass ratio of 1:2. The resulting mixed solution is mixed with calcium peroxide in a mass ratio of 1:1 to obtain a mixture 2.
[0055] PEG and xanthan gum were stirred and mixed and dissolved in deionized water at room temperature, wherein the concentration of PEG in the solution was 10 wt % and the concentration of xanthan gum was 0.1%, and then the mixture was uniformly mixed with calcium peroxide at a mass ratio of 1:1 to obtain a mixture 3.
[0056] In a three-layer co-extrusion unit containing three single-screw extruders, mixtures 1, 2, and 3 are extruded separately, and compounded in a single-hole die. Extrusion molding obtains a three-layer extruded material strip with a diameter of 20 mm, with mixture 1 in the center and a thickness of 10 mm, a middle layer of mixture 2 and a thickness of 6 mm, and a surface layer of mixture 3 and a thickness of 4 mm. The extruded material strip is cut into a column with a length of 10 mm at the exit of the die, and then immediately frozen at -20°C for 8 hours, then thawed for 4 hours, and then frozen again. After repeating this process 3 times, the final product is obtained.
[0057] Embodiment 5:
[0058] The PVA particles were dissolved in deionized water at 80-95° C. with stirring to prepare a 10 wt % PVA solution (embedding solution 1), cooled to room temperature, and then mixed with calcium peroxide at a mass ratio of 1:1 to obtain a mixture 1.
[0059] PVA particles are dissolved in deionized water at 80-95°C with stirring to prepare a 2wt% PVA solution, which is then cooled to room temperature. PEG and xanthan gum are then stirred and mixed and dissolved in deionized water at room temperature. The PEG concentration in the solution is 10wt%, and the xanthan gum concentration is 0.05%. The solution is stirred and mixed with the 2wt% PVA solution in a mass ratio of 1:2. The resulting mixed solution is mixed with calcium peroxide in a mass ratio of 1:1 to obtain a mixture 2.
[0060] PEG and xanthan gum were stirred and mixed and dissolved in deionized water at room temperature, wherein the concentration of PEG in the solution was 10 wt % and the concentration of xanthan gum was 0.1%, and then the mixture was uniformly mixed with calcium peroxide at a mass ratio of 1:1 to obtain a mixture 3.
[0061] In a three-layer co-extrusion unit containing three single-screw extruders, mixtures 1, 2, and 3 are extruded separately, and compounded in a single-hole die. Extrusion molding is performed to obtain a three-layer extruded material strip with a diameter of 20 mm, with mixture 1 in the center and a thickness of 8 mm, mixture 2 in the middle and a thickness of 6 mm, and mixture 3 in the surface and a thickness of 8 mm. The extruded material strip is cut into a column with a length of 10 mm at the exit of the die, and then immediately frozen at -20°C for 8 hours, then thawed for 4 hours, and then frozen again. After repeating this process 3 times, the final product is obtained.
[0062] Comparative example:
[0063] The PVA particles were dissolved in deionized water at 80-95° C. under stirring to prepare a PVA solution with a concentration of 10 wt %, which was then cooled to room temperature and mixed with calcium peroxide at a mass ratio of 1:1 to obtain a mixture 1.
[0064] The mixture 1 was extruded through a single screw extruder at room temperature to obtain an extruded material strip with a diameter of 20 mm. The extruded material strip was cut into columns with a length of 10 mm at the place leaving the head of the extruder. It was then immediately frozen at -20°C for 8 hours, thawed for 4 hours, and frozen again. This process was repeated 3 times to obtain the final product.
[0065] Test results - oxygen release experiments of oxygen release agents of Examples 1-5 and Comparative Examples:
[0066] Boil deionized water and add it to a sealed container, making sure the container is full of water, then blow nitrogen for 10 minutes to remove the remaining dissolved oxygen in the water, insert a dissolved oxygen test electrode into the container to monitor the dissolved oxygen value (DO) online, weigh a certain amount of oxygen release agent, add it to the container and seal it, and monitor the change of DO over time online at normal temperature and pressure. The oxygen release curve is shown in Figure 1 The oxygen release rate of the comparative example is obviously slower at the initial stage of administration, while the embodiment has a faster oxygen release rate at the initial stage of administration and can maintain a very long oxygen release time.
[0067] The specific implementation modes of the present invention are described above, but the present invention is not limited thereto. The present invention can also have various changes without departing from the purpose of the present invention.
Claims
1. A gradually disintegrating slow-release oxygen composite material, characterized in that: It consists of three layers: inner core layer, middle layer and surface layer. The material of the inner core layer is calcium peroxide and physically cross-linked PVA; The materials of the intermediate layer are calcium peroxide, water-soluble substances and water-insoluble substances; The materials of the surface layer are calcium peroxide and water-soluble substances.
2. The gradually disintegrating slow-release oxygen composite material according to claim 1, characterized in that: The calcium peroxide content of the core material is 30-80wt%, and / or The content of polyvinyl alcohol is 20-70wt%, and the alcoholysis degree of polyvinyl alcohol is above 99%.
3. The gradually disintegrating slow-release oxygen composite material according to claim 1, characterized in that: The non-water-soluble substance in the middle layer is physically cross-linked PVA, and the water-soluble substance in the middle layer includes a water-soluble binder and a thickener, wherein the water-soluble binder is polyethylene glycol, and the thickener is xanthan gum or sodium alginate.
4. The gradually disintegrating and sustained-release oxygen composite material according to claim 1 or 3, characterized in that: The materials of the intermediate layer include the following components:
5. The gradually disintegrating slow-release oxygen composite material according to claim 1, characterized in that: The water-soluble substance of the surface layer includes a water-soluble binder and a thickener, wherein the water-soluble binder is polyethylene glycol, and the thickener is xanthan gum or sodium alginate.
6. The gradually disintegrating and sustained-release oxygen composite material according to claim 1 or 5, characterized in that: The material of the surface layer includes the following components: Calcium peroxide 40-80%; Polyethylene glycol 20-60wt%; Xanthan gum or sodium alginate 0-1wt%.
7. The gradually disintegrating slow-release oxygen composite material according to claim 1, characterized in that: The gradually disintegrating slow-release oxygen composite material is in the form of a column with a diameter of 5-25 mm and a length of 10-20 mm, preferably a diameter of 10-12 mm; The thickness of the inner core layer is 2-8 mm, the thickness of the middle layer is 5-10 mm, and the thickness of the surface layer is 2-10 mm. Preferably, the thickness of the inner core layer is 3-5 mm, the thickness of the middle layer is 5-6 mm, and the thickness of the surface layer is 2-5 mm.
8. A method for preparing a gradually disintegrating slow-release oxygen composite material, characterized in that: The following steps are involved: Preparation of inner core layer material: PVA particles are dissolved in deionized water under stirring at 80-95° C., the mass concentration of the PVA aqueous solution is 5-20%, the completely dissolved PVA solution is cooled to room temperature, and then cooled to 0-10° C. under refrigeration conditions, which is recorded as embedding solution 1; calcium peroxide is added to the embedding solution 1, and mechanically stirred and mixed evenly, the stirring time is 5-20 minutes, and the stirring speed is 100-300 rpm, to obtain a flowable paste, which is recorded as mixture 1, and the mixture 1 is extruded by a single screw extruder to obtain the inner core layer material; Preparation of the intermediate layer material: PVA particles are dissolved in deionized water under stirring conditions at 80-95° C., and the mass concentration of the PVA aqueous solution is 2-10%; polyethylene glycol, xanthan gum or sodium alginate are dissolved in deionized water under stirring and mixing at room temperature to form a mixed solution, and the mixed solution is stirred and mixed with the PVA solution at room temperature in a certain proportion, which is recorded as embedding solution 2; calcium peroxide is added to the embedding solution 2, and stirred and mixed evenly, the stirring time is 5-20 minutes, and the stirring speed is 100-300rpm, to obtain a flowable paste, which is recorded as mixture 2, and the mixture 2 is extruded by a single screw extruder to prepare the intermediate layer material; Preparation of surface layer material: polyethylene glycol, xanthan gum or sodium alginate are stirred and dissolved in deionized water at room temperature to obtain a mixed solution, which is recorded as embedding solution 3; calcium peroxide is added to the embedding solution 3, and stirred and mixed evenly for 5-20 minutes at a stirring speed of 100-300 rpm to obtain a flowable paste, which is recorded as mixture 3; a single-screw extruder is used to extrude mixture 3 to prepare the surface layer material; Material compounding: The materials of the inner core layer, the middle layer and the surface layer are compounded in a single-hole die head and extruded to obtain a three-layer extruded material strip with a diameter of 5-25 mm. The center of the material strip is mixture 1, the middle layer is mixture 2, and the surface layer is mixture 3. The composite extrudate is cut at the extruder head to obtain a column with a length of 10-20 mm, which is then immediately frozen at -20°C for 8-12 hours, then thawed for 4 hours, and then frozen again. This is repeated 2-4 times to obtain the final product.
9. The method for preparing the gradually disintegrating and slowly releasing oxygen composite material according to claim 8, characterized in that: In the preparation of the core layer material, the PVA concentration is preferably 8-10wt%, and / or The completely dissolved PVA solution is preferably cooled to 5°C under refrigeration, and / or The mass ratio of calcium peroxide to embedding solution 1 is 1:1-1:
3.
10. The method for preparing the gradually disintegrating and slowly releasing oxygen composite material according to claim 8, characterized in that: In the preparation of the intermediate layer material, the concentration of polyethylene glycol in the mixed solution is 2-15wt%, the concentration of xanthan gum or sodium alginate is 0-2wt%, wherein the concentration of polyethylene glycol solution is preferably 5-10wt%, the concentration of xanthan gum or sodium alginate is preferably 0-0.5wt%, and / or The mixing mass ratio of the mixed solution to the PVA solution is 1:1-1:5; and / or The mass ratio of calcium peroxide to embedding solution 2 is 1:1-1:
3.
11. The method for preparing the gradually disintegrating and slowly releasing oxygen composite material according to claim 8, characterized in that: In the preparation of the surface material, the concentration of polyethylene glycol in the mixed solution is 5-20wt%, and the concentration of xanthan gum or sodium alginate is 0-2wt%, wherein the concentration of polyethylene glycol solution is preferably 5-10wt%, and the concentration of xanthan gum or sodium alginate is preferably 0-0.5wt%; and / or The mass ratio of calcium peroxide to embedding solution 3 is 1:1-1:3.
Citation Information
Patent Citations
Slow-release oxygen cation crosslinker and preparation method thereof
CN109574184A
Production method of calcium peroxide particles for slowly releasing oxygen
CN110184072A
Composite material for removing alga-derived odorous substances in black and odorous water, and preparation method and application thereof
CN110745998A
Measuring apparatus for subscriber, and control method thereof
KR102159685B1
Cited By
River and lake bottom mud in-situ integrated purification system and construction method thereof
CN119591297A
In-situ integrated purification system for river and lake sediment and construction method thereof
CN119591297B
Gradient oxygen release material with multi-layer core-shell structure as well as preparation method and application of gradient oxygen release material
CN122007136A