Electromagnetic shielding type conductive flexible stone-like facing patch and preparation method thereof

By adjusting the component ratio and modifying the graphene and carbon nanotubes, a conductive composite material is formed, which solves the problem of excessive use of graphene and poor dispersion effect in flexible imitation stone veneers, and realizes conductivity and electromagnetic shielding. Improvement ensures the flexibility and corrosion resistance of the product.

CN118878249APending Publication Date: 2024-11-01RONGXIN (TANGSHAN) COATINGS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410898625.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Since the aggregate accounts for a large proportion of existing flexible imitation stone veneers and the matrix resin does not have electrical conductivity, the graphene is used too much, the color is inaccurate, and the dispersion effect is poor, which affects flexibility and processability, and is prone to erosion. Extraction.

Method used

Using component A and component B with a volume ratio of 30-40:1, water-soluble polyvinyl alcohol and aniline derivative monomer are added to component A, and conductive composite materials are added to component B, through carboxyl groups, graphene and carbon nanotubes are passed through carboxyl groups. The conductive composite material is formed by synchronous ultrasonic and high-speed shearing treatment, and is evenly dispersed in the matrix resin, reducing the amount of graphene, and improving conductivity and electromagnetic shielding.

Benefits of technology

The amount of conductive composite material is significantly reduced, ensuring that it is evenly dispersed in flexible stone imitation finish patches, maintaining flexibility and processability, and improving corrosion resistance and electromagnetic shielding effect to avoid corrosion and extraction of conductive composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878249A_ABST
    Figure CN118878249A_ABST
Patent Text Reader

Abstract

The invention provides an electromagnetic shielding type conductive flexible stone-like facing patch and a preparation method thereof. The electromagnetic shielding type conductive flexible stone-like facing patch comprises aggregate, a component A and a component B, the component A comprises water-soluble polyvinyl alcohol, a water-soluble aniline derivative monomer, hydrochloric acid, an initiator, methacrylic acid, styrene, methyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl amino acrylate, acetoacetoxy ethyl methacrylate, monobutyl itaconate, an ethylene-vinyl acetate copolymer and deionized water; the component B comprises zinc acetate, ammonia water, a conductive composite material, water-soluble polyvinyl alcohol and deionized water, and the conductive composite material is prepared by mixing graphene and carbon nanotubes in a weight ratio of 1: (0.5-2.5) and sequentially performing carboxylation modification and amination modification. The electromagnetic shielding type conductive flexible stone-like facing patch provided by the invention has conductivity and electromagnetic shielding functions, and can be used as a building wall decoration material in the fields of medical treatment, industry, airports, military facilities, aerospace and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to an electromagnetic shielding type conductive flexible imitation stone facing patch and a preparation method thereof. Background Art

[0002] Flexible imitation stone veneer patch, also known as soft stone or soft stone, is made of inorganic mineral powders such as mineral soil, ore, and mineral powder as the main materials, and a small amount of water-based polymer is added as a modifier. It is formed at low temperature through molecular structure modification and reorganization. It has a very high degree of stone simulation in appearance, and has the advantages of fast production cycle, safety and environmental protection, no risk of separation, light weight, aging resistance, acid and alkali resistance, freeze-thaw resistance, and low construction cost. The inventor has proposed a flexible imitation stone veneer sheet and its preparation method (China Invention Patent Application No. 202010499907.2, Application Publication No. CN 111635163 A), which comprises aggregate and component A and component B in a volume ratio of (90-105):3, 60-80 parts by weight of aggregate are added to every 25-30 parts by weight of component A, and the aggregate is a mixture of 100-150 mesh natural colored sand and 50-80 mesh natural colored sand in a mass ratio of 1:(0.1-0.5); the component A comprises the following raw materials in weight: 1-3 parts of water-soluble polyvinyl alcohol, 0.13-0.33 parts of potassium persulfate, 10.5-21 parts of deionized water, 0.8-2.8 parts of methacrylic acid, 0.1-0.5 parts of styrene, 1-3 parts of methyl methacrylate 1-4 parts of ethyl methacrylate, 2-5 parts of isooctyl acrylate, 0.5-4 parts of isooctyl methacrylate, 0.1-0.5 parts of ethyl acetoacetate methacrylate, 1.8-3.5 parts of ethylene-vinyl acetate copolymer; the component B includes the following raw materials by weight: 2-4 parts of zinc acetate, 1-2 parts of ammonia water, 0.1-1 parts of water-soluble polyvinyl alcohol and 60-100 parts of deionized water, and the concentration of the ammonia water is 25%; during preparation, first add aggregate to component A and stir until uniform, then add component B dropwise, vibrate and exhaust, cross-link and cure at 120-160°C for 10-15 minutes, then demold and trim to shape. Compared with the prior art, the flexible imitation stone veneer sheet has good flexibility, can bend against the surface of a cylinder with a diameter of 10-20mm without cracks on the surface, has many usage scenarios and is easy to construct, and is especially suitable for pasting special parts with curvature.

[0003] Graphene is a nanomaterial composed of carbon atoms in sp2 hybrid orbitals and has a two-dimensional hexagonal honeycomb lattice. It has good chemical stability and excellent electrical conductivity. In the prior art, graphene is often added as a conductive filler to a matrix resin to make a conductive coating to meet the decorative needs of buildings in the electronic, communication, industrial, medical, military and other technical fields that require the ability to conduct current and dissipate static electricity. To this end, the applicant tried to add graphene to the above-mentioned flexible imitation stone veneer sheet in order to obtain a flexible imitation stone veneer patch with conductivity. However, the applicant found that: since the proportion of aggregate in the sheet is relatively large and the matrix resin is not conductive, in order to achieve the ideal conductive effect, a large amount of graphene is used. A large amount of graphene will cause the following problems: (1) The color of the patch is darker. After adding pigment in actual production, the final color of the patch is quite different from the expected color; (2) A large amount of graphene is easy to agglomerate in the matrix resin, the dispersion effect is not good, and the compatibility with the matrix resin is poor and the adhesion is not strong, which not only affects the flexibility and processability of the patch, but also is easily eroded and extracted.

[0004] To this end, this application is filed. Summary of the invention

[0005] In order to solve the above technical problems, the present invention proposes an electromagnetic shielding conductive flexible stone-like veneer patch and a preparation method thereof.

[0006] The technical solution of the present invention is achieved in this way:

[0007] On the one hand, the present invention provides an electromagnetic shielding conductive flexible imitation stone veneer patch, comprising aggregate and component A and component B in a volume ratio of (30-40):1, wherein 2-3 times the weight of the component A is added to each 1 weight part of the component A, and the aggregate is a mixture of 100-150 mesh natural colored sand and 50-80 mesh natural colored sand in a mass ratio of 1:(0.1-0.5);

[0008] Every 100 parts by weight of the component A comprises the following raw materials in parts by weight: 3-9 parts of water-soluble polyvinyl alcohol, 4.5-8.5 parts of water-soluble aniline derivative monomer, 2-4.5 parts of hydrochloric acid, 0.45-1.5 parts of initiator, 2.4-7.1 parts of methacrylic acid, 3.5-6.8 parts of styrene, 4-8 parts of methyl methacrylate, 4.5-7.6 parts of isooctyl acrylate, 1.5-7.2 parts of isooctyl aminoacrylate, 0.5-1.5 parts of ethyl acetoacetate methacrylate, 0.2-0.8 parts of monobutyl itaconate, 6-10 parts of ethylene-vinyl acetate copolymer, and the rest is deionized water; the concentration of the hydrochloric acid does not exceed 2 mol / L;

[0009] Every 100 parts by weight of the component B comprises the following raw materials in parts by weight: 2-4 parts of zinc acetate, 2-4 parts of ammonia water, 15-30 parts of a conductive composite material, 0.5-2 parts of a water-soluble polyvinyl alcohol, and the rest is deionized water, wherein the concentration of the ammonia water is 25%, and the conductive composite material is prepared by mixing graphene and carbon nanotubes in a weight ratio of 1:(0.5-2.5) and sequentially performing carboxyl modification and amino modification.

[0010] The component A and the component B of the present invention are stored separately, preferably sealed and stored in a ventilated and dry indoor environment, and are mixed and stirred evenly when used. After mixing, a zinc ion cross-linked core-shell acrylic ionomer emulsion is formed, and the acrylic ionomer emulsion contains a water-soluble polyaniline derivative. Under the modification effect of the water-soluble polyaniline derivative, the acrylic ionomer emulsion has certain conductivity and electromagnetic shielding properties after being cured into a film. Since the component B contains a conductive composite material, it synergizes with the conductive matrix resin, so that the finally obtained flexible imitation stone veneer patch has certain electromagnetic shielding and conductive functions, and the polyaniline derivative also has excellent environmental stability, which is helpful to improve corrosion resistance.

[0011] Compared with the prior art, the present invention significantly reduces the amount of conductive composite material used. The conductive composite material dispersed in a small amount, evenly and stably in the matrix resin neither affects the color adjustment of the flexible imitation stone veneer patch nor affects its flexibility and processability, and the conductive composite material is not easily corroded and extracted.

[0012] On the basis of the above, in order to meet the needs of actual applications, inorganic pigments and / or organic pigments can be added in appropriate amounts to component A or component B, preferably component A, so that the color of the flexible imitation stone veneer patch is diversified, and the addition of pigments will not affect the electromagnetic shielding effect of the product. Even the addition of certain inorganic pigments such as iron oxide green may help to enhance the electromagnetic shielding effect of the product.

[0013] Furthermore, the initiator is compounded by potassium persulfate and ammonium persulfate in a weight ratio of 1:(0.21-0.42).

[0014] Potassium persulfate is mainly used as a polymerization initiator for acrylic monomers, with high initiation efficiency and greater solubility at high temperatures; ammonium persulfate has a lower initiation efficiency than potassium persulfate, and its solubility at high temperatures is also slightly poor. The applicant unexpectedly discovered that a small amount of ammonium persulfate and potassium persulfate compounding can help water-soluble polyaniline derivatives and acrylic ionomers form a network structure, thereby increasing the cross-linking density and adhesion of the matrix resin. It is speculated that this may be because the primary free radicals generated by the thermal grading of ammonium persulfate and the monomers open double bonds to form monomer free radicals, and then through the polymerization reaction and the bifunctional group effect of the network agent, the polymer chains are linked to form a network structure, and there are a variety of resins with different molecular weights in the system, and the small molecule resins are effectively filled between the macromolecular resins, which ultimately makes the flexible imitation stone veneer patch flexible, dense, and has strong adhesion, preventing the infiltration of corrosive chemicals, and making the conductive composite material not easily corroded and extracted.

[0015] Furthermore, every 100 parts by weight of component A further comprises 3.8-6.7 parts by weight of a perfluoroalkylethyl acrylate monomer, wherein the perfluoroalkylethyl acrylate monomer is at least one of perfluorobutylethyl acrylate, perfluorohexylethyl acrylate, and perfluorooctylethyl acrylate.

[0016] After the perfluoroalkylethyl acrylate monomers are polymerized, fluorinated acrylic polymers are formed. This is attributed to the fact that the fluorinated side chains of the polymers extend into the air and occupy the interface between the polymer and the air during the film-forming and drying process, and are largely located on the surface of the coating, thus shielding and protecting the CC main chain. The resulting fluorinated acrylic polymers have many excellent surface properties, such as low surface energy, low friction, stain resistance, good water resistance, oil resistance, weather resistance, and chemical corrosion resistance, which can further improve the performance of flexible imitation stone veneer patches.

[0017] Specifically, the ethylene-vinyl acetate copolymer is an ethylene-vinyl acetate copolymer having a vinyl acetate mass percentage of 20%-25%, the water-soluble polyvinyl alcohol is polyvinyl alcohol 1788, and the water-soluble aniline derivative monomer is at least one of N-propanesulfonic acid aniline, o-aminobenzenesulfonic acid, and m-aminobenzenesulfonic acid.

[0018] On the other hand, the present invention provides a method for preparing an electromagnetic shielding conductive flexible imitation stone veneer patch, comprising the following preparation steps:

[0019] (1) dissolving a quaternary ammonium salt in deionized water to obtain a saturated quaternary ammonium salt dispersion, then adding graphene oxide, ultrasonically exfoliating, and then adding carbon nanotubes, continuing ultrasonication and mechanical stirring, centrifugally filtering, placing in a mixed solution of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1, reflux at 60-65° C. for at least 3 hours, cooling to room temperature, washing to neutrality, filtering, and vacuum drying to obtain a carboxylation product; mixing the obtained carboxylation product with polyethyleneimine and deionized water and ultrasonically dispersing, then stirring and reacting at 320-350° C. for 5-8 hours under nitrogen gas conditions for amination treatment, filtering, and drying to obtain a conductive composite material;

[0020] (2) adding water-soluble polyvinyl alcohol and 1 / 3 of the initiator to 2 / 3 of deionized water and stirring at 80-85° C. for at least 10 minutes to obtain a first solution, adding 1 / 3 of the initiator to 1 / 3 of the deionized water and stirring to obtain a second solution, then adding the second solution, 1 / 2 of the methacrylic acid and styrene to the first solution, stirring for a first polymerization reaction for at least 30 minutes; adding water-soluble aniline derivative monomer, methyl methacrylate, isooctyl acrylate, isooctyl aminoacrylate, ethyl acetoacetate methacrylate, monobutyl itaconate, ethylene-vinyl acetate copolymer, hydrochloric acid and 1 / 2 of methacrylic acid to the product obtained in the previous step, stirring to obtain a uniform mixture, continuing to stir at 85-88° C. and dripping 1 / 3 of the initiator to carry out a second polymerization reaction, and continuing to react for 2-5 hours after the dripping is completed, and before adding the ethylene-vinyl acetate copolymer, the ethylene-vinyl acetate copolymer is pre-irradiated with β rays in an air atmosphere using an electron accelerator, the pre-irradiation dose is 20-30 kGy, and the pre-irradiation time is 5-15 minutes;

[0021] (3) zinc acetate, ammonia water, water-soluble polyvinyl alcohol and deionized water are mixed and stirred uniformly, and then a conductive composite material is added thereto, and synchronous ultrasonic and high-speed shear treatment is performed. After the synchronous ultrasonic and high-speed shear treatment, the two-dimensional sheet-like graphene and the one-dimensional tubular carbon nanotubes form a highly uniform aqueous carbon slurry;

[0022] (4) Add the aggregate to the product obtained in step (2), stir mechanically until uniform, and then dropwise add the product obtained in step (3) under continuous mechanical stirring. After the dropwise addition is completed, continue mechanical stirring for at least 1 hour and then apply it to the mold with a coating thickness of 3-5 mm. After vibration and exhaust, cross-link and cure at 120-145° C. for 10-15 minutes, then demold and perform post-processing.

[0023] In this embodiment, in step (1), the graphene oxide and carbon nanotubes dispersed with quaternary ammonium salt have positive charges on their surfaces. Therefore, when carboxylation treatment is performed, they adsorb with negatively charged carboxyl groups, and the carboxylation modification effect is better. On this basis, amino modification is performed. The two chemical modifications make the surface have more active groups. These active groups can provide more reaction sites for subsequent cross-linking reactions and help improve the dispersibility and stability of graphene and carbon nanotubes in the system.

[0024] In this embodiment, in step (2), methacrylic acid and styrene are used as core monomers, methyl methacrylate, isooctyl acrylate, isooctyl aminoacrylate, ethyl acetoacetate methacrylate, monobutyl itaconate, ethylene-vinyl acetate copolymer, and methacrylic acid are used as shell monomers, and deionized water is used as solvent. Copolymerization is initiated in the presence of an initiator to obtain a core-shell acrylic ionomer emulsion, which is then copolymerized with a zinc-ammine complex to obtain a zinc ion cross-linked core-shell acrylic ionomer emulsion. In this process, a water-soluble aniline derivative monomer is added to the shell monomer, which is copolymerized under the action of an initiator to obtain a water-soluble polyaniline derivative. The water-soluble polyaniline derivative is not only conductive, but also forms a nanofiber multilayer structure under the doping of hydrochloric acid, which is conducive to the multiple reflection and loss of electromagnetic waves, thereby making the resin matrix conductive and electromagnetic shielding. In addition, the polyaniline derivative can also repair chemical aging, making the product have better corrosion resistance, and objectively further avoiding the conductive composite material from being extracted due to corrosion; isooctyl acrylate and isooctyl aminoacrylate are soft monomers that can improve weather resistance and softness; ethyl methacrylate and monobutyl itaconate are functional crosslinkers. The cross-linking monomer contains a variety of active groups, and the synergistic effect can provide a variety of cross-linking points for the cross-linking reaction, thereby improving the adhesion of the polymer; the ethylene-vinyl acetate copolymer is a viscous elastomeric material, and the flexibility of the film can be improved after the film is formed, and after pre-irradiation, the ethylene-vinyl acetate copolymer produces a macromolecular peroxide, which can be used as an initiator in the polymerization reaction, so that it is grafted with part of the monomers in the above-mentioned acrylic ester, and the grafted product can significantly improve the toughness, elasticity and impact resistance of the emulsion after curing; in component A, the hard monomer, soft monomer and functional cross-linking monomer of the polymerization reaction are properly proportioned, and the synergistic effect helps to improve the ductility of the emulsion, and finally a dense, flexible and breathable film is obtained.

[0025] In this embodiment, in step (3), since the conductive composite material is modified by amino, it has good compatibility with component B and can exist stably for a long time. Component B has good uniformity and can be maintained stably for a long time.

[0026] In this embodiment, in step (4), at 120-145° C., the solvent water in component A and component B is evaporated, the functional groups previously isolated by water come into contact with each other, and a comprehensive cross-linking reaction occurs rapidly and then solidifies; post-processing includes but is not limited to trimming, coating, drying, stamping, lamination, etc.

[0027] The quaternary ammonium salt is dissolved in deionized water to obtain a saturated quaternary ammonium salt dispersion, and then graphene oxide is added first, and carbon nanotubes are added after ultrasonic exfoliation, and ultrasonic and mechanical stirring are continued. After centrifugal filtration, it is placed in a mixed solution of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1, and refluxed at 60-65° C. for at least 3 hours. After cooling to room temperature, it is washed to neutrality, filtered, and vacuum dried; the obtained product is mixed with polyethyleneimine and deionized water and ultrasonically dispersed, and then nitrogen is passed through the mixture to react at 320-350° C. for 5-8 hours with stirring, filtered, and dried to obtain a conductive composite material;

[0028] Specifically, in step (1), the weight of polyethyleneimine is 1-2 times the total weight of graphene oxide and carbon nanotubes, and the weight of deionized water is 3-5 times the total weight of graphene oxide and carbon nanotubes.

[0029] In this embodiment, the amount of polyethyleneimine and deionized water should not be too little or too much. If the amount of polyethyleneimine is too little or too little deionized water, the amination of graphene oxide and carbon nanotubes is not good. If the amount of polyethyleneimine is too much or too much deionized water is too much, although the amination effect is good, the subsequent separation takes a long time and the separation efficiency is low, so that the preparation of the conductive composite material takes a long time and the production efficiency is low. When the above amount is used, a win-win situation of amination effect and production efficiency can be achieved.

[0030] Specifically, in step (3), the synchronous ultrasound and high-speed shear treatment is specifically performed as follows: ultrasound is performed at a power of not less than 500 W, a frequency of not less than 50 Hz, and an amplitude of not less than 50 μm for at least 2 hours, and shear stirring is performed synchronously at 2000-2500 r / min during this process.

[0031] The graphene and carbon nanotubes that have been dispersed, carboxylated, and amino-modified have a variety of active groups on their surfaces. These active groups: (1) improve the uniformity of the dispersion of the conductive composite material in deionized water, so that the conductive composite material is evenly dispersed and fully covers the entire system; (2) promote the curing of the acrylic resin, which shrinks when it cures, so that the evenly dispersed graphene and carbon nanotubes are close to and in contact with each other, forming a multi-dimensional, maze-like conductive channel; (3) enhance the original π-π electron interaction between graphene, carbon nanotubes, and water-soluble aniline derivative monomers, so that the water-soluble aniline derivatives are adsorbed on the surface of the conductive composite material to form an electromagnetic shielding coating, which further improves the uniformity of dispersion and the adhesion to the resin matrix. , and solves the problem of poor conductivity of conductive composite materials during functional modification in the prior art. Graphene and carbon nanotubes are filling composite electromagnetic shielding materials, polyaniline derivatives are intrinsic conductive polymers, and the coexistence of multiple conductors diversifies the carrier transmission channels and electromagnetic shielding methods. In short, water-soluble polyaniline derivatives constitute a conductive substrate, and graphene and carbon nanotubes with polyaniline derivatives adsorbed on the surface form multi-dimensional, maze-like conductive channels and electromagnetic shielding channels. Multiple conductors enrich the carrier transmission channels and electromagnetic shielding methods, making the carrier movement smoother and the electromagnetic shielding effect more significant. The synergistic effect of the three makes the generated flexible imitation stone veneer patch have certain conductivity and electromagnetic shielding properties.

[0032] It should be noted that synchronous ultrasound and high-speed shear treatment are essential steps in this preparation method. Without synchronous ultrasound and high-speed shear treatment, it is difficult to obtain a water-based carbon slurry with good uniformity by general mechanical stirring, and thus it is impossible to form a conductive channel with stable structure, uniform conductivity and obvious electromagnetic shielding effect.

[0033] Specifically, in step (1), during the first polymerization reaction, a perfluoroalkyl ethyl acrylate monomer is also added, and the perfluoroalkyl ethyl acrylate monomer is at least one of perfluorobutyl ethyl acrylate, perfluorohexyl ethyl acrylate, and perfluorooctyl ethyl acrylate.

[0034] In order to further improve the weather resistance of the obtained flexible imitation stone veneer patch, it is preferred to add perfluoroalkyl ethyl acrylate monomers with good compatibility with the system during the first polymerization reaction. The perfluoroalkyl ethyl acrylate monomers are added to the first solution at the same time as the second solution, 1 / 2 of methacrylic acid, and styrene, and work together with the hard monomers methyl methacrylate and styrene to effectively reduce the damage to the patch by water and other chemical liquids, increase the hardness of the flexible imitation stone veneer patch, and further improve the weather resistance of the flexible imitation stone veneer patch.

[0035] Specifically, a layer of base material is laid at 1 / 3-1 / 2 of the mold. The base material is a grid-shaped substrate made of non-woven fabric, glass cloth or synthetic resin. When casting the film, part of the material is poured into the mold first. The upper surface of the material is slightly higher than the base material. The material is vibrated to exhaust the air first, and then the remaining material is poured in. The material is vibrated again to exhaust the air and then cross-linked and cured.

[0036] Specifically, after coating and pressing, a release layer is formed on the upper surface of the material, and the release layer is any one of PET, PP, and PE release films.

[0037] In summary, the electromagnetic shielding conductive flexible imitation stone facing patch proposed in the present invention has the characteristics of absorbing, conducting and attenuating electromagnetic waves, and can be used as a building wall decoration material in the fields of medical, industrial, airport, military facilities, aerospace, etc. (the construction method is no different from the existing flexible facing bricks, and the specific details can refer to the prior art shown in the background technology). It has a certain degree of shielding electromagnetic waves, protecting internal equipment from electromagnetic wave interference and sensitive information from being leaked, and ensuring the normal operation of key equipment and the communication quality; its preparation method is easy to operate and implement, with a short cross-linking and curing time and low temperature, and is environmentally friendly, energy-saving, and efficient, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a photo of the product obtained in Example 1;

[0039] Figure 2 This is a construction drawing of the product obtained in Example 1 used for exterior wall finishing of a building. DETAILED DESCRIPTION

[0040] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] The materials used in the following examples and comparative examples are all commercially available, and the specific manufacturers are not limited. The following examples and comparative examples use: the aggregate is a mixture of 100-150 mesh natural colored sand and 50-80 mesh natural colored sand in a mass ratio of 1:0.3; the ethylene-vinyl acetate copolymer is an ethylene-vinyl acetate copolymer with a vinyl acetate mass percentage of 25%; and the water-soluble polyvinyl alcohol is polyvinyl alcohol 1788. The specific operations of carboxyl modification and amino modification of the conductive composite material are as follows: dissolve hexadecyltrimethylammonium bromide in deionized water to form a saturated dispersion, then add graphene oxide, ultrasonically exfoliate at a power of 100W for 30 minutes, then add carbon nanotubes, continue ultrasonication and mechanical treatment at the same power for 45 minutes, centrifuge and filter, place in a mixed solution of concentrated sulfuric acid (mass fraction 98%) and concentrated nitric acid (mass fraction 68%) in a volume ratio of 3:1, reflux at 62°C for 5 hours, cool to room temperature, wash with water and ethanol to neutrality, filter, and vacuum dry at no higher than 45°C; mix the obtained product with polyethyleneimine and deionized water and ultrasonically disperse at a power of 100W for 35 minutes, then stir and react at 349°C for 7 hours with nitrogen, filter, and dry.

[0042] Example 1

[0043] An electromagnetic shielding conductive flexible imitation stone veneer patch, comprising aggregate, component A and component B;

[0044] Every 100 parts by weight of component A comprises the following raw materials in parts by weight: 5.8 parts of water-soluble polyvinyl alcohol, 6.1 parts of N-propanesulfonic acid aniline, 3.2 parts of hydrochloric acid with a concentration of 2 mol / L, 1.2 parts of initiator, 5.0 parts of methacrylic acid, 5.2 parts of styrene, 6 parts of methyl methacrylate, 5.8 parts of isooctyl acrylate, 4.7 parts of isooctyl aminoacrylate, 1.0 part of ethyl acetoacetate methacrylate, 0.5 part of monobutyl itaconate, 8.0 parts of ethylene-vinyl acetate copolymer, 5.1 parts of perfluorobutyl ethyl acrylate, and the rest is ionized water, and 1.2 parts of initiator contain 0.92 parts of potassium persulfate and 0.28 parts of ammonium persulfate;

[0045] The preparation method of component A is as follows: water-soluble polyvinyl alcohol and 0.4 parts of initiator are added to 2 / 3 of deionized water and stirred at 83°C for 15 minutes to obtain a first solution, 0.4 parts of initiator are added to 1 / 3 of deionized water and stirred evenly to obtain a second solution, then the second solution, 2.5 parts of methacrylic acid and styrene are added to the first solution, and the first polymerization reaction is carried out under stirring for 45 minutes; N-propanesulfonic acid aniline, methyl methacrylate, isooctyl acrylate are added to the product obtained in the previous step; Ester, isooctyl aminoacrylate, ethyl acetoacetate methacrylate, monobutyl itaconate, ethylene-vinyl acetate copolymer, perfluorobutyl ethyl acrylate, hydrochloric acid and 2.5 parts of methacrylic acid, stir evenly, continue stirring at 85°C and drop 0.4 parts of initiator for the second polymerization, continue the reaction for 4 hours after the drop addition, and before adding the ethylene-vinyl acetate copolymer, use an electron accelerator to pre-irradiate with β rays in an air atmosphere, the pre-irradiation dose is 26 kGy, and the pre-irradiation time is 12 minutes;

[0046] Every 100 parts by weight of component B includes the following raw materials in parts by weight: 3 parts of zinc acetate, 3 parts of ammonia water, 24 parts of conductive composite material, 1.2 parts of water-soluble polyvinyl alcohol, and the rest is deionized water, the concentration of ammonia water is 25%, and the conductive composite material is prepared by mixing graphene and carbon nanotubes in a weight ratio of 1:1.5 and sequentially performing carboxyl modification and amino modification;

[0047] The preparation method of component B is as follows: zinc acetate, ammonia water, water-soluble polyvinyl alcohol and deionized water are mixed and stirred evenly, and then the conductive composite material is added thereto, and finally ultrasonicated for 3 hours at a power of 800 W, a frequency of 100 Hz and an amplitude of 200 μm, and shear stirring is performed synchronously at 2300 r / min during the process;

[0048] Add 2.5 times the weight of component A to component A, stir mechanically until uniform, then add component B dropwise while stirring mechanically, the volume ratio of component A to component B is 35:1, continue to stir mechanically for 2 hours after the addition is completed, then apply and press into a mold with a depth of 4 mm and cover with a PET film, a grid-like substrate made of a non-woven fabric base material is laid at a depth of 2 mm in the mold, half of the material is poured into the mold when casting the film, the upper surface of the material is slightly higher than the base material, vibrate to exhaust first, and then continue to pour the remaining half of the material, vibrate to exhaust again and cross-link and cure, and demold after cross-linking and curing at 130°C for 12 minutes.

[0049] Example 2

[0050] Compared with Example 1, perfluorobutyl ethyl acrylate is not added to component A, and the rest is the same as Example 1.

[0051] Example 3

[0052] Compared with Example 1, the perfluorobutyl ethyl acrylate in component A is adjusted to an equal weight portion of perfluorohexyl ethyl acrylate, and the rest is the same as Example 1.

[0053] Example 4

[0054] Compared with Example 1, the perfluorobutyl ethyl acrylate in component A is adjusted to an equal weight portion of perfluorooctyl ethyl acrylate, and the rest is the same as Example 1.

[0055] Example 5

[0056] Compared with Example 1, the initiator in component A does not contain ammonium persulfate, but is entirely composed of potassium persulfate.

[0057] Example 6

[0058] Compared with Example 1, the initiator in component A does not contain potassium persulfate, but is entirely composed of ammonium persulfate.

[0059] Example 7

[0060] Compared with Example 1, the N-propanesulfonic acid aniline in component A is adjusted to an equal weight portion of anthranilic acid, and the rest is the same as Example 1.

[0061] Example 8

[0062] Compared with Example 1, the N-propanesulfonic acid aniline in component A is adjusted to an equal weight portion of m-aminobenzenesulfonic acid, and the rest is the same as Example 1.

[0063] Example 9

[0064] Compared with Example 1, the component types of component A remain unchanged, but the content is changed, specifically: every 100 parts by weight of component A includes the following raw materials in parts by weight: 9 parts of water-soluble polyvinyl alcohol, 6.1 parts of water-soluble aniline derivative monomer, 2 parts of hydrochloric acid, 1.5 parts of initiator, 5 parts of methacrylic acid, 3.5 parts of styrene, 8 parts of methyl methacrylate, 5.2 parts of isooctyl acrylate, 1.5 parts of isooctyl aminoacrylate, 1.5 parts of ethyl acetoacetate methacrylate, 0.5 parts of monobutyl itaconate, 6 parts of ethylene-vinyl acetate copolymer, and the rest is deionized water.

[0065] Example 10

[0066] Compared with Example 1, the component types of component A remain unchanged, but the content is changed. Specifically, every 100 parts by weight of component A includes the following raw materials in parts by weight: 3 parts of water-soluble polyvinyl alcohol, 8.5 parts of water-soluble aniline derivative monomer, 3.2 parts of hydrochloric acid, 0.45 parts of initiator, 7.1 parts of methacrylic acid, 5.0 parts of styrene, 4 parts of methyl methacrylate, 7.6 parts of isooctyl acrylate, 3.2 parts of isooctyl aminoacrylate, 0.5 parts of ethyl acetoacetate methacrylate, 0.8 parts of monobutyl itaconate, 8 parts of ethylene-vinyl acetate copolymer, and the rest is deionized water.

[0067] Embodiment 11

[0068] Compared with Example 1, the component types of component A remain unchanged, but the content is changed. Specifically, every 100 parts by weight of component A includes the following raw materials in parts by weight: 6 parts of water-soluble polyvinyl alcohol, 4.5 parts of water-soluble aniline derivative monomer, 4.5 parts of hydrochloric acid, 0.8 parts of initiator, 2.4 parts of methacrylic acid, 6.8 parts of styrene, 6 parts of methyl methacrylate, 4.5 parts of isooctyl acrylate, 7.2 parts of isooctyl aminoacrylate, 1 part of ethyl acetoacetate methacrylate, 0.2 parts of monobutyl itaconate, 10 parts of ethylene-vinyl acetate copolymer, and the rest is deionized water.

[0069] Example 12

[0070] Compared with Example 1, the component types of component B remain unchanged, but the content is changed. Specifically, every 100 parts by weight of component B includes the following raw materials in parts by weight: 3 parts of zinc acetate, 2 parts of ammonia water, 30 parts of conductive composite material, 1.2 parts of water-soluble polyvinyl alcohol, and the rest is deionized water. The concentration of the ammonia water is 25%. The conductive composite material is formed by mixing graphene and carbon nanotubes in a weight ratio of 1:0.5 and sequentially performing carboxyl modification and amino modification.

[0071] Embodiment 13

[0072] Compared with Example 1, the component types of component B remain unchanged, but the content is changed. Specifically, every 100 parts by weight of component B includes the following raw materials in parts by weight: 4 parts of zinc acetate, 3 parts of ammonia water, 15 parts of conductive composite material, 2 parts of water-soluble polyvinyl alcohol, and the rest is deionized water. The concentration of ammonia water is 25%. The conductive composite material is formed by mixing graphene and carbon nanotubes in a weight ratio of 1:1.8 and sequentially performing carboxyl modification and amino modification.

[0073] Embodiment 14

[0074] Compared with Example 1, the component types of component B remain unchanged, but the content is changed. Specifically, every 100 parts by weight of component B includes the following raw materials in parts by weight: 2 parts of zinc acetate, 4 parts of ammonia water, 22 parts of conductive composite materials, 0.5 parts of water-soluble polyvinyl alcohol, and the rest is deionized water. The concentration of ammonia water is 25%. The conductive composite material is formed by mixing graphene and carbon nanotubes in a weight ratio of 1:2.5 and sequentially performing carboxyl modification and amino modification.

[0075] Comparative Example 1

[0076] Compared with Example 1, N-propanesulfonic acid aniline is not added to component A, and the rest is the same as Example 1.

[0077] Comparative Example 2

[0078] Compared with Example 1, no conductive composite material is added to Component B, and the rest is the same as Example 1.

[0079] Comparative Example 3

[0080] Compared with Example 1, the conductive composite material added to component B is composed of graphene and carbon nanotubes in a weight ratio of 1:1.5, but the conductive composite material is neither carboxyl-modified nor amino-modified.

[0081] Comparative Example 4

[0082] Compared with Example 1, the conductive composite material added to component B is composed of graphene and carbon nanotubes in a weight ratio of 1:1.5, and the conductive composite material is only carboxylated but not aminolated.

[0083] Comparative Example 5

[0084] Compared with Example 1, the conductive composite material added to component B is composed of graphene and carbon nanotubes in a weight ratio of 1:1.5, and the conductive composite material is not carboxylated but only amino-modified.

[0085] Comparative Example 6

[0086] Compared with Example 1, when preparing component B, after the conductive composite material is added, ultrasound is not performed, and shear stirring is performed at 2300 r / min. The rest is the same as Example 1.

[0087] Comparative Example 7

[0088] Compared with Example 1, when preparing component B, after the conductive composite material is added, ultrasound is only performed for 3 hours at a power of 800 W, a frequency of 100 Hz, and an amplitude of 200 μm without shear stirring. The rest is the same as Example 1.

[0089] Comparative Example 8

[0090] Compared with Example 1, N-propanesulfonic acid aniline is not added to component A, and conductive composite material is not added to component B. The rest is the same as Example 1.

[0091] The products obtained in each embodiment have a dense texture, good flexibility and a high similarity to stone in appearance. Taking Example 1 as an example, the appearance of the obtained product is as follows: Figure 1 As shown in the figure, when it is used as a decorative material for the exterior wall of a building close to the substation, the actual decorative effect is as follows Figure 2 As shown, the decorative effect is basically the same as that of stone.

[0092] The products obtained from all the above embodiments are made into sheets of corresponding specifications and tested for performances 1-8 according to the provisions of JG / T 540-2017 for flexible imitation stone facing materials for buildings (specific test data are shown in Table 1 below). The appearance, flexibility, heating dimensional change rate, temperature change resistance, stain resistance, chemical corrosion resistance, resistance to artificial climate change, and salt spray resistance of each product fully meet the requirements of W-type products. In addition, the adhesion of performance 9 is tested according to GB / T9286-1998 paint film adhesion determination method-cross-cut test of paint and varnish film, and the adhesion of each embodiment is level 0; performance 10, a 30-micron thick paint film is made and its square resistance value is tested by the four-probe method. The square resistance value of each embodiment is 0.5-2KΩ. Among them, the conductivity of Example 1 is the best, and its square resistance value is as low as 0.5KΩ. The electromagnetic shielding properties of the products obtained from each embodiment were measured according to the method specified in SJ20524-1995. Each embodiment showed good electromagnetic shielding effect, among which Embodiment 1 was the best. After actual measurement, when the frequency of the electromagnetic wave was 30, 100, 300, 500, and 1000 Hz, the corresponding shielding effects were 70, 68, 65, 60, and 50 dB, respectively. Regardless of whether it was a low-frequency electromagnetic wave or a high-frequency electromagnetic wave, it had a good shielding effect.

[0093] By further comparing the appearance of the products obtained in various embodiments, the applicant found that: compared with Embodiment 2, Embodiment 5, and Embodiment 6, the product obtained in Embodiment 1 is denser. After further testing, its flexibility, chemical resistance, and artificial aging resistance are also better. When its flexibility is tested, it can bend closely to the surface of a 40-50mm cylinder without cracks. There is no change after soaking in 10% sulfuric acid, 10% sodium hydroxide, and 10% ammonia water for 10 days. In the 100-day artificial accelerated aging test, its surface has no powdering, cracking, or shedding.

[0094]

[0095] Similarly, the conductivity of each comparative example was tested using the same method. The block resistance values ​​of comparative examples 1 to 7 were 200KΩ, 300KΩ, 105KΩ, 80KΩ, 85KΩ, 176KΩ, and 204KΩ, respectively. Comparative example 8 exceeded the range and could not be measured, which shows that its resistance value is very large and has no conductivity. From the above block resistance value test results, it can be seen that when N-propanesulfonic acid aniline is not added to component A and conductive composite material is not added to component B, the resulting product does not have conductivity and electromagnetic shielding function. When N-propanesulfonic acid aniline is added to component A and conductive composite material is not added to component B, or conductive composite material is added to component B and N-propanesulfonic acid aniline is not added to component A, the resulting product has a certain conductivity, but the conductive effect is far less than when N-propanesulfonic acid aniline and conductive composite material are added at the same time. Further, if the conductive composite material is not subjected to carboxylation or amino modification or only one of the modifications is performed, the effect of improving the conductivity of the product after addition is not good; if the conductive composite material is not subjected to synchronous ultrasound and high-speed shearing treatment or only one of the modifications is performed after addition, the effect of improving the conductivity of the product is also unsatisfactory. From the comparison of Comparative Examples 1 to Comparative Examples 7 with Example 1, the reason why the products obtained by the present invention have good conductivity and electromagnetic shielding properties is the result of the synergistic effect of many technical parameters. The polyaniline derivative, the conductive composite, the carboxylation and amino modification of the conductive composite, and the synchronous ultrasound and high-speed shearing treatment after the conductive composite is added are all very important for improving the conductivity of the product. The absence of any step will result in the product failing to achieve the best conductivity.

[0096] To sum up: the electromagnetic shielding conductive flexible stone-like veneer patch prepared by the preparation method proposed in the present invention, the filling composite electromagnetic shielding material and the intrinsic conductive polymer therein work together to reflect and guide the electromagnetic energy flow, and will generate current and magnetic polarization opposite to the source electromagnetic field inside it. When it is used as an interior wall decoration material, it can effectively weaken the outward radiation of internal electromagnetic waves. When it is used as an exterior wall decoration material, it can effectively weaken the inward radiation of external electromagnetic waves. Therefore, it can be widely used as a wall decoration material with conductive function and the ability to weaken electromagnetic radiation in large and medium-sized industrial computer rooms such as hospitals, telecommunications, community substations, computer rooms, etc.

[0097] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention. The components or connection methods not specifically described in the present invention adopt the existing technology. The front side, rear side, left side, and right side described in the present invention are for the convenience of describing its structure and are not intended to limit the protection scope of the present invention.

Claims

1. An electromagnetic shielding conductive flexible imitation stone veneer patch, characterized in that: The invention comprises aggregate and component A and component B in a volume ratio of (30-40):1, wherein 2-3 times the weight of the component A is added to each weight of the component A, and the aggregate is a mixture of 100-150 mesh natural colored sand and 50-80 mesh natural colored sand in a mass ratio of 1:(0.1-0.5); Every 100 parts by weight of the component A comprises the following raw materials in parts by weight: 3-9 parts of water-soluble polyvinyl alcohol, 4.5-8.5 parts of water-soluble aniline derivative monomer, 2-4.5 parts of hydrochloric acid, 0.45-1.5 parts of initiator, 2.4-7.1 parts of methacrylic acid, 3.5-6.8 parts of styrene, 4-8 parts of methyl methacrylate, 4.5-7.6 parts of isooctyl acrylate, 1.5-7.2 parts of isooctyl aminoacrylate, 0.5-1.5 parts of ethyl acetoacetate methacrylate, 0.2-0.8 parts of monobutyl itaconate, 6-10 parts of ethylene-vinyl acetate copolymer, and the rest is deionized water; the concentration of the hydrochloric acid does not exceed 2 mol / L; Every 100 parts by weight of the component B comprises the following raw materials in parts by weight: 2-4 parts of zinc acetate, 2-4 parts of ammonia water, 15-30 parts of a conductive composite material, 0.5-2 parts of a water-soluble polyvinyl alcohol, and the rest is deionized water, wherein the concentration of the ammonia water is 25%, and the conductive composite material is prepared by mixing graphene and carbon nanotubes in a weight ratio of 1:(0.5-2.5) and sequentially performing carboxyl modification and amino modification.

2. The electromagnetic shielding conductive flexible imitation stone veneer patch according to claim 1, characterized in that: The initiator is prepared by compounding potassium persulfate and ammonium persulfate in a weight ratio of 1:(0.21-0.42).

3. The electromagnetic shielding conductive flexible imitation stone veneer patch according to claim 1, characterized in that: Every 100 parts by weight of the component A further comprises 3.8-6.7 parts by weight of a perfluoroalkylethyl acrylate monomer, wherein the perfluoroalkylethyl acrylate monomer is at least one of perfluorobutylethyl acrylate, perfluorohexylethyl acrylate and perfluorooctylethyl acrylate.

4. The electromagnetic shielding conductive flexible imitation stone veneer patch according to any one of claims 1 to 3, characterized in that: The ethylene-vinyl acetate copolymer is an ethylene-vinyl acetate copolymer with a vinyl acetate mass percentage of 20%-25%, the water-soluble polyvinyl alcohol is polyvinyl alcohol 1788, and the water-soluble aniline derivative monomer is at least one of N-propanesulfonic acid aniline, o-aminobenzenesulfonic acid, and m-aminobenzenesulfonic acid.

5. A method for preparing the electromagnetic shielding conductive flexible imitation stone veneer patch according to any one of claims 1 to 4, characterized in that: The method comprises the following preparation steps: (1) dissolving a quaternary ammonium salt in deionized water to obtain a saturated quaternary ammonium salt dispersion, then adding graphene oxide, ultrasonically exfoliating, and then adding carbon nanotubes, continuing ultrasonication and mechanical stirring, centrifugally filtering, placing in a mixed solution of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1, reflux at 60-65° C. for at least 3 hours, cooling to room temperature, washing to neutrality, filtering, and vacuum drying; mixing the obtained product with polyethyleneimine and deionized water and ultrasonically dispersing, then stirring and reacting at 320-350° C. for 5-8 hours under nitrogen, filtering, and drying to obtain a conductive composite material; (2) adding water-soluble polyvinyl alcohol and 1 / 3 of the initiator to 2 / 3 of deionized water and stirring at 80-85° C. for at least 10 minutes to obtain a first solution, adding 1 / 3 of the initiator to 1 / 3 of the deionized water and stirring to obtain a second solution, then adding the second solution, 1 / 2 of the methacrylic acid and styrene to the first solution, stirring for a first polymerization reaction for at least 30 minutes; adding water-soluble aniline derivative monomer, methyl methacrylate, isooctyl acrylate, isooctyl aminoacrylate, ethyl acetoacetate methacrylate, monobutyl itaconate, ethylene-vinyl acetate copolymer, hydrochloric acid and 1 / 2 of methacrylic acid to the product obtained in the previous step, stirring to obtain a uniform mixture, continuing to stir at 85-88° C. and dropping 1 / 3 of the initiator to carry out a second polymerization, and continuing to react for 2-5 hours after the addition is completed, and before adding the ethylene-vinyl acetate copolymer, the ethylene-vinyl acetate copolymer is pre-irradiated with β rays in an air atmosphere using an electron accelerator, the pre-irradiation dose is 20-30 kGy, and the pre-irradiation time is 5-15 minutes; (3) zinc acetate, ammonia water, water-soluble polyvinyl alcohol and deionized water are mixed and stirred uniformly, and then a conductive composite material is added thereto, and ultrasonic and high-speed shear treatment is performed simultaneously; (4) Add the aggregate to the product obtained in step (2), stir mechanically until uniform, and then dropwise add the product obtained in step (3) under continuous mechanical stirring. After the dropwise addition is completed, continue mechanical stirring for at least 1 hour and then apply it to the mold with a coating thickness of 3-5 mm. After vibration and exhaust, cross-link and cure at 120-145° C. for 10-15 minutes, then demold and perform post-processing.

6. The method for preparing the electromagnetic shielding conductive flexible imitation stone veneer patch according to claim 5, characterized in that: In step (1), the weight of polyethyleneimine is 1-2 times the total weight of graphene oxide and carbon nanotubes, and the weight of deionized water is 3-5 times the total weight of graphene oxide and carbon nanotubes.

7. The method for preparing the electromagnetic shielding conductive flexible imitation stone veneer patch according to claim 5, characterized in that: In step (3), the specific operation of the synchronous ultrasound and high-speed shear treatment is: ultrasound at a power of not less than 500 W, a frequency of not less than 50 Hz, and an amplitude of not less than 50 μm for at least 2 hours, and during this process, shear stirring is synchronously performed at 2000-2500 r / min.

8. The method for preparing the electromagnetic shielding conductive flexible imitation stone veneer patch according to claim 5, characterized in that: In step (1), during the first polymerization reaction, a perfluoroalkyl ethyl acrylate monomer is further added, and the perfluoroalkyl ethyl acrylate monomer is at least one of perfluorobutyl ethyl acrylate, perfluorohexyl ethyl acrylate, and perfluorooctyl ethyl acrylate.

9. The method for preparing the electromagnetic shielding conductive flexible imitation stone veneer patch according to any one of claims 6 to 8, characterized in that: A layer of base material is laid at 1 / 3-1 / 2 of the mold. The base material is a grid-like substrate made of non-woven fabric, glass cloth or synthetic resin. When casting the film, part of the material is poured into the mold first, and the upper surface of the material is slightly higher than the base material. The material is vibrated to exhaust the air first, and then the remaining material is poured in. The material is vibrated again to exhaust the air and then cross-linked and cured.

10. The method for preparing the electromagnetic shielding conductive flexible imitation stone veneer patch according to claim 9, characterized in that: After coating, a release layer is formed on the upper surface of the material. The release layer is any one of PET, PP, and PE release films.