Preparation method and application of rigid-tough balanced nucleating agent

By using norbornene diacid anhydride and amine substances in polypropylene to react with metal oxides, the problems of rigidity and toughness balance of polypropylene are solved, and the performance improvement and processing stability of polypropylene are achieved sex.

CN118878434APending Publication Date: 2024-11-01NORTH HUAJIN CHEM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411071128.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The prior art is difficult to achieve a balance between rigidity and toughness in polypropylene, and it is often necessary to add a variety of nucleating agents, resulting in reduced use effect and uncertainty in subsequent processing.

Method used

By reacting norbornene diacid anhydride with an amine substance to form amide acid and reacting with the first main group metal oxide, a rigid and tough equilibrium nucleating agent that can synergistically induce polypropylene to form α and β crystal forms is prepared.

Benefits of technology

The coordinated improvement between the rigidity and toughness of polypropylene is achieved, and the impact strength, flexural modulus and thermal deformation temperature are improved. At the same time, it is non-toxic, environmentally friendly, low-cost, and simple formula.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878434A_ABST
    Figure CN118878434A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of nucleating agents, and particularly discloses a preparation method and application of a rigid-tough balanced nucleating agent. According to the nucleating agent, norbornene dianhydride reacts with amines to generate norbornene amic acid with amide groups, the norbornene amic acid reacts with salts of first main group metal elements to generate norbornene amic acid salt, and beta crystals generated through induction of the amide groups and alpha crystals generated through induction of dicarboxylic acid monovalent metal groups have a synergistic effect; the impact strength, the bending modulus and the thermal deformation temperature of the polypropylene are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nucleating agents, and specifically discloses a preparation method of a rigid-tough balanced nucleating agent and application thereof. Background Art

[0002] The high performance of polypropylene by nucleating agents is mainly achieved by regulating its microstructure during the crystallization process. Microstructure determines macroscopic performance. Polypropylene is a semi-crystalline polymer with a complex polycrystalline structure. Under different processing conditions, five different forms of spherulite structures, namely α, β, γ, δ and pseudo-hexagonal, can be generated. In different crystal structures, the mutual arrangement between the spherulite morphology and its lamellar structure is very different. The size and morphology of the spherulite have an important influence on the macroscopic mechanical and optical properties of the material. For example, the mechanical and optical properties of α-type and β-type polypropylene are different. The spherulites of α-type polypropylene are positive spherulites with small birefringence; β-type polypropylene is negative spherulites with large birefringence and colorful butterfly shape. The macroscopic properties of the two types of spherulite polypropylene are also very different. The mutual arrangement between the spherulite morphology and lamellar structure of different crystal structures is very different, so they have different processing and application properties.

[0003] α-crystal nucleating agent can increase the rigidity of polypropylene by providing nucleation points in the crystallization process of polypropylene, so that polypropylene can crystallize at a higher temperature, thereby increasing the crystallization temperature of polypropylene, reducing the size of spherulites, and making the spherulites more perfect, but the toughness of polypropylene will decrease; β-crystal nucleating agent can induce polypropylene to form β-crystal, and the characteristic of β-crystal of polypropylene is to improve the toughness and heat deformation temperature of polypropylene, but it is not conducive to the rigidity of polypropylene. Therefore, how to balance the rigidity and toughness of polypropylene has become a key issue.

[0004] Therefore, it is necessary to develop a rigidity-toughness balanced nucleating agent to solve the above problems, as the current means for achieving the rigidity-toughness balance of polypropylene are to add two or more different types of nucleating agents and to use α and β nucleating agents in combination. The two substances will affect each other, reduce the effect of use, and bring more uncertainty to the subsequent processing and use of the polymer. Summary of the invention

[0005] The technical solution adopted by the present invention is as follows:

[0006] In a first aspect, the present invention provides a method for preparing a rigid-tough balanced nucleating agent, which specifically comprises the following steps: adding nadic anhydride to an ester solvent to obtain a mixed solution, dropping an amine substance into the mixed solution, reacting at 40 to 60° C. to obtain an amide acid precipitate, filtering, washing and drying the amide acid precipitate; using water as a solvent, reacting the obtained amide acid with a first main group metal oxide under heating conditions of 60 to 80° C. to obtain a rigid-tough balanced nucleating agent;

[0007] The molar ratio of the nadic anhydride to the amine substance is 1:1 to 1:1.5; the molar ratio of the amic acid to the first main group metal oxide is 1:0.2 to 1:1; the amount of the solvent water added is 2 to 5 times the mass of the amic acid precipitate;

[0008] The amine substance is one of benzylidene amine and dodecylamine;

[0009] Preferably, the first main group metal oxide is one of lithium oxide, sodium oxide and potassium oxide.

[0010] Preferably, the ester solvent is ethyl acetate, and the concentration of nadic anhydride in the ethyl acetate solvent is 5 to 15 mol / L.

[0011] Preferably, the molar ratio of the amic acid to the first main group metal oxide is 1:0.5.

[0012] Preferably, the amount of solvent water added is 4 times the mass of the amic acid precipitate.

[0013] In a second aspect, the present invention provides a rigid-tough balanced nucleating agent, which is prepared by the method described in the first aspect.

[0014] Preferably, the rigid-tough balanced nucleating agent is any one of bicyclo[2.2.1]heptene-2-benzylamide-3-carboxylate lithium, bicyclo[2.2.1]heptene-2-benzylamide-3-carboxylate sodium, bicyclo[2.2.1]heptene-2-benzylamide-3-carboxylate potassium, bicyclo[2.2.1]heptene-2-dodecylamide-3-carboxylate lithium, bicyclo[2.2.1]heptene-2-dodecylamide-3-carboxylate sodium, and bicyclo[2.2.1]heptene-2-dodecylamide-3-carboxylate potassium.

[0015] In a third aspect, the present invention provides a use of the rigidity-toughness balanced nucleating agent described in the second aspect in polypropylene, for improving the impact strength, flexural modulus and heat deformation temperature of polypropylene.

[0016] Preferably, the rigid-tough balanced nucleating agent is added to polypropylene at a concentration of 0.1 wt% to 0.3 wt%.

[0017] Furthermore, after adding the antioxidant, the acid absorbent and the nucleating agent, the polypropylene is mixed and stirred evenly in a high-speed mixer, and then extruded and granulated by a twin-screw extruder.

[0018] Beneficial effects achieved by the present invention:

[0019] The invention uses nadic anhydride and amines to react to generate namic acid with an amide group, and then reacts with salts of the first main group metal element to generate namic acid salt, wherein the amide group can induce polypropylene to form a β crystal form, and the monovalent dicarboxylic acid group can induce polypropylene to form an α crystal form, and the two crystal forms synergistically achieve the rigidity and toughness balance of polypropylene. The nucleating agent of the invention is non-toxic and tasteless, environmentally friendly, has high addition efficiency, good dispersibility, and low cost. The nucleating agent has a simple formula when used in polypropylene, and no other modified monomers are added except for an antioxidant, an acid absorber, and a nucleating agent, so that the performance of polypropylene is effectively maintained to be stable. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The infrared detection results of the nucleating agents obtained in Examples 1-3 of the present invention;

[0021] Figure 2 These are the infrared detection results of the nucleating agents obtained in Examples 4-6 of the present invention. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail in conjunction with the following examples. It should be noted that the present invention is not limited to the following examples.

[0023] Example 1

[0024] 1 mol of nadic anhydride and 100 ml of ethyl acetate were added to the first reaction kettle, and after stirring and dissolving, 1.2 mol of benzylamine was added dropwise to the reactant, and the mixture was reacted at 50° C. for 60 min to obtain a precipitate of naphthalene benzamide acid. The precipitate was filtered, washed, and dried to obtain 250 g of naphthalene benzamide acid. 1000 ml of deionized water was added to the second reaction kettle as a solvent, and the obtained 250 g of naphthalene benzamide acid was mixed with 13.77 g of lithium oxide by stirring, and the mixture was reacted at 70° C. for 30 min to obtain 235.4 g of bicyclo[2.2.1]heptene-2-benzoic acid amine-3-carboxylic acid lithium, with a yield of 92.14%.

[0025] Example 2

[0026] 1 mol of nadic anhydride and 100 ml of ethyl acetate were added to the first reaction kettle, and after stirring and dissolving, 1.2 mol of benzylamine was added dropwise to the reactant, and the mixture was reacted at 50° C. for 60 min to obtain a precipitate of nadic acid. The precipitate was filtered, washed, and dried to obtain 250 g of nadic acid. 1000 ml of deionized water was added to the second reaction kettle as a solvent, and the obtained 250 g of nadic acid was mixed with 28.55 g of sodium oxide by stirring, and the mixture was reacted at 70° C. for 30 min to obtain 251.3 g of sodium bicyclo[2.2.1]heptene-2-benzylamide-3-carboxylate, with a yield of 92.98%.

[0027] Example 3

[0028] 1 mol of nadic anhydride and 100 ml of ethyl acetate were added to the first reaction kettle, and after stirring and dissolving, 1.2 mol of benzylamine was added dropwise to the reactant, and the mixture was reacted at 50° C. for 60 min to obtain naphthalene benzamide acid. The precipitate was filtered, washed and dried to obtain 250 g of naphthalene benzamide acid. 1000 ml of deionized water was added to the second reaction kettle as a solvent, and the obtained 250 g of naphthalene benzamide acid was mixed with 43.40 g of potassium oxide by stirring, and the mixture was reacted at 70° C. for 30 min to obtain 264.3 g of bicyclo[2.2.1]heptene-2-benzylamide-3-carboxylate potassium, with a yield of 92.70%.

[0029] Example 4

[0030] 1 mol of naphthalene anhydride and 100 ml of ethyl acetate were added to the first reaction kettle, and after stirring and dissolving, 1.2 mol of dodecylamine was added dropwise to the reactant, and the mixture was reacted at 50° C. for 60 min to obtain 318.05 g of naphthalene benzamide acid, and the precipitate was filtered, washed and dried; 1272 ml of deionized water was added to the second reaction kettle as a solvent, and the obtained 318.05 g of naphthalene dodecamide acid was mixed with 13.60 g of lithium oxide by stirring, and the mixture was reacted at 70° C. for 30 min to obtain 298.6 g of bicyclo[2.2.1]heptene-2-dodecanoic acid amine-3-carboxylic acid lithium, with a yield of 92.3%.

[0031] Example 5

[0032] 1 mol of naphthalene anhydride and 100 ml of ethyl acetate were added to the first reaction kettle, and after stirring and dissolving, 1.2 mol of dodecylamine was added dropwise to the reactant, and the mixture was reacted at 50° C. for 60 min to obtain 318.05 g of naphthalene benzamide acid. The precipitate was filtered, washed and dried. 1272 ml of deionized water was added to the second reaction kettle as a solvent, and the obtained 318.05 g of naphthalene dodecamide acid was mixed with 28.20 g of sodium oxide by stirring, and the mixture was reacted at 70° C. for 30 min to obtain 315.01 g of sodium bicyclo[2.2.1]heptene-2-dodecanoic acid amine-3-carboxylate, with a yield of 93.2%.

[0033] Example 6

[0034] 1 mol of nadic anhydride and 100 ml of ethyl acetate were added to the first reaction kettle, and after stirring and dissolving, 1.2 mol of dodecylamine was added dropwise to the reactant, and the mixture was reacted at 50° C. for 60 min to obtain 318.05 g of naphthalene benzamide acid, and the precipitate was filtered, washed and dried; 1272 ml of deionized water was added to the second reaction kettle as a solvent, and the obtained 318.05 g of naphthalene dodecamide acid was mixed with 42.86 g of potassium oxide by stirring, and the mixture was reacted at 70° C. for 30 min to obtain 324.50 g of bicyclo[2.2.1]heptene-2-dodecanoic acid amine-3-carboxylate potassium, with a yield of 92.00%.

[0035] Test Example 1

[0036] The bicyclo[2.2.1]heptene-2-benzylamine-3-carboxylate lithium, bicyclo[2.2.1]heptene-2-benzylamine-3-carboxylate sodium, bicyclo[2.2.1]heptene-2-benzylamine-3-carboxylate potassium, bicyclo[2.2.1]heptene-2-dodecylamine-3-carboxylate lithium, bicyclo[2.2.1]heptene-2-dodecylamine-3-carboxylate sodium, bicyclo[2.2.1]heptene-2-dodecylamine-3-carboxylate prepared in Examples 1-6 were mixed with dicyclo[2.2.1]heptene-2-dodecylamine-3-carboxylate sodium, dicyclo[2.2.1]heptene-2-dodecylamine-3-carboxylate potassium. 3g of each of potassium and 1000g of homopolypropylene F401 were added, and then 1000ppm of antioxidant 1010, 1000ppm of antioxidant 168 and 800ppm of acid absorbing agent hydrotalcite DHT-4A were added, mixed and stirred evenly in a high-speed mixer, and then extruded and granulated by a twin-screw extruder, and the temperature zones were 190℃, 210℃, 210℃, and 190℃, respectively, and then injection molded to obtain standard specimens, marked as serial numbers 1-1 to 1-6. At the same time, homopolypropylene F401 without adding nucleating agent was also extruded and granulated with the same amount of antioxidant and acid absorbing agent to prepare specimens, marked as serial numbers 0-1.

[0037] Test Example 2

[0038] The bicyclo[2.2.1]heptene-2-benzylamine-3-carboxylate lithium, bicyclo[2.2.1]heptene-2-benzylamine-3-carboxylate sodium, bicyclo[2.2.1]heptene-2-benzylamine-3-carboxylate potassium, bicyclo[2.2.1]heptene-2-dodecylamine-3-carboxylate lithium, bicyclo[2.2.1]heptene-2-dodecylamine-3-carboxylate sodium, bicyclo[2.2.1]heptene-2-dodecylamine-3-carboxylate prepared in Examples 1-6 were mixed with dicyclo[2.2.1]heptene-2-dodecylamine-3-carboxylate sodium, dicyclo[2.2.1]heptene-2-dodecylamine-3-carboxylate potassium. 6 g of each of potassium was added to 3000 g of homopolypropylene F401, and then 1000 ppm of antioxidant 1010, 1000 ppm of antioxidant 168 and 800 ppm of acid absorber hydrotalcite DHT-4A were added, mixed and stirred evenly in a high-speed mixer, and then extruded into granules by a twin-screw extruder. The temperature zones were 190°C, 210°C, 210°C and 190°C respectively, and then injection molding was performed to obtain standard specimens, which were marked as serial numbers 2-1 to 2-6.

[0039] Test Example 3

[0040] The bicyclo[2.2.1]heptene-2-benzylamine-3-carboxylate lithium, bicyclo[2.2.1]heptene-2-benzylamine-3-carboxylate sodium, bicyclo[2.2.1]heptene-2-benzylamine-3-carboxylate potassium, bicyclo[2.2.1]heptene-2-dodecylamine-3-carboxylate lithium, bicyclo[2.2.1]heptene-2-dodecylamine-3-carboxylate sodium, bicyclo[2.2.1]heptene-2-dodecylamine-3-carboxylate potassium synthesized in Examples 1-6 were added. 3g of each was added to 3000g of copolymerized polypropylene PPB240, and then 1000ppm antioxidant 1010, 1000ppm antioxidant 168 and 800ppm acid absorbing agent hydrotalcite DHT-4A were added, mixed and stirred evenly in a high-speed mixer, and then extruded and granulated by a twin-screw extruder, with each temperature zone being 200℃, 220℃, 220℃, and 200℃, and then injection molded to obtain standard specimens, marked as serial numbers 3-1 to 3-6. At the same time, homopolymerized polypropylene PPB240 without adding nucleating agent was also extruded and granulated with the same amount of antioxidant and acid absorbing agent to prepare specimens, marked as serial numbers 0-2.

[0041] Test Example 4

[0042] The bicyclo[2.2.1]heptene-2-dodecanoic acid amine-3-carboxylic acid lithium, bicyclo[2.2.1]heptene-2-benzylamine-3-carboxylic acid sodium, bicyclo[2.2.1]heptene-2-benzylamine-3-carboxylic acid potassium, bicyclo[2.2.1]heptene-2-dodecanoic acid amine-3-carboxylic acid lithium, bicyclo[2.2.1]heptene-2-dodecanoic acid amine-3-carboxylic acid sodium, bicyclo[2.2.1]heptene-2-dodecanoic acid amine-3-carboxylic acid 6g of each of potassium and 1010 were added to 3000g of copolymerized polypropylene PPB240, and then 1000ppm of antioxidant 1010, 1000ppm of antioxidant 168 and 800ppm of acid absorbent hydrotalcite DHT-4A were added, mixed and stirred evenly in a high-speed mixer, and then extruded and granulated by a twin-screw extruder, with the temperature zones being 200℃, 220℃, 220℃ and 200℃ respectively, and then injection molded to obtain standard specimens, marked as serial numbers 4-1 to 4-6.

[0043] Comparative Example 1

[0044] 1.5 g of each commercially available α-nucleating agent NA-11 and commercially available β-nucleating agent TMB-5 were added simultaneously to 3000 g of copolymerized polypropylene F401, and then 1000 ppm of antioxidant 1010, 1000 ppm of antioxidant 168 and 800 ppm of acid absorber hydrotalcite DHT-4A were added. After mixing and stirring evenly in a high-speed mixer, the mixture was extruded and granulated through a twin-screw extruder. The temperature zones were 200°C, 220°C, 220°C and 200°C respectively, and then injection molding was performed to obtain standard specimens.

[0045] Comparative Example 2

[0046] 3 g of each commercially available α-nucleating agent NA-11 and commercially available β-nucleating agent TMB-5 were added simultaneously to 3000 g of copolymerized polypropylene F401, and then 1000 ppm of antioxidant 1010, 1000 ppm of antioxidant 168 and 800 ppm of acid absorber hydrotalcite DHT-4A were added. After mixing and stirring evenly in a high-speed mixer, the mixture was extruded and granulated through a twin-screw extruder. The temperature zones were 200°C, 220°C, 220°C and 200°C respectively, and then injection molding was performed to obtain standard specimens.

[0047] Comparative Example 3

[0048] 1.5 g of each commercially available α-nucleating agent NA-11 and commercially available β-nucleating agent TMB-5 were added simultaneously to 3000 g of copolymerized polypropylene PPB240, and then 1000 ppm of antioxidant 1010, 1000 ppm of antioxidant 168 and 800 ppm of acid absorber hydrotalcite DHT-4A were added. After mixing and stirring evenly in a high-speed mixer, the mixture was extruded and granulated through a twin-screw extruder. The temperature zones were 200°C, 220°C, 220°C and 200°C respectively, and then injection molding was performed to obtain standard specimens.

[0049] Comparative Example 4

[0050] 3 g of each commercially available α-nucleating agent NA-11 and commercially available β-nucleating agent TMB-5 were added simultaneously to 3000 g of copolymerized polypropylene PPB240, and then 1000 ppm of antioxidant 1010, 1000 ppm of antioxidant 168 and 800 ppm of acid absorber hydrotalcite DHT-4A were added. After mixing and stirring evenly in a high-speed mixer, the mixture was extruded and granulated through a twin-screw extruder. The temperature zones were 200°C, 220°C, 220°C and 200°C respectively, and then injection molding was performed to obtain standard specimens.

[0051] Test Results

[0052] The test of nucleating agent modified polypropylene is carried out according to GB 2918-1998 (Standard Environment for Conditioning and Testing of Plastic Specimens) at (23±2)°C and relative humidity (RH) of (50±5)%, and the specimen conditioning time is 48h. The physical property tests are carried out according to national standards: the notched impact strength of the cantilever beam is carried out according to the standard ASTM D-256, the flexural modulus is carried out according to the standard ASTM D-790, and the heat deformation temperature is carried out according to the standard ASTM D648. The test results are listed in the table below.

[0053] Figure 1 Infrared detection results of Example 1-3: at 1654cm -1 There is an amide C=O stretching vibration absorption peak at 1400cm-1, a -COO- symmetric vibration absorption peak at 1577cm-1, and a -1 There is a -COO- antisymmetric vibration absorption peak at , which proves that the synthesized product is a monovalent salt of amide acid.

[0054] Figure 2 Infrared detection results of Example 4-6: at 1637cm -1 There is an amide C=O stretching vibration absorption peak at 1407cm-1, a -COO- symmetric vibration absorption peak at 1554cm-1, and a -1 There is a -COO- antisymmetric vibration absorption peak at , which proves that the synthesized product is a monovalent salt of amide acid.

[0055] Table 1 Results of different rigidity-toughness balance nucleating agents for modifying homopolymer polypropylene F401 (addition amount 0.1%)

[0056] Serial number Impact strength J / m Flexural modulus / MPa Heat deformation temperature / ℃ 0-1 F401 without nucleating agent 32.72 1293.515 98.9 1-1 Test Example 1 76.52 1390.63 105.8 1-2 Test Example 1 72.08 1321.26 104.1 1-3 Test Example 1 71.56 1357.05 102.1 1-4 Test Example 1 62.11 1421.05 109.8 1-5 Test Example 1 66.03 1496.36 108.6 1-6 Test Example 1 62.44 1461.03 107.3

[0057] Compared with 0-1 to 2-6, the rigidity-toughness balance nucleating agent can effectively improve the impact performance, flexural modulus and heat deformation temperature of F401.

[0058] Table 2 Results of different rigidity-toughness balance nucleating agents for modifying homopolymer polypropylene F401 (addition amount 0.2%)

[0059] Serial number Impact strength J / m Flexural modulus / MPa Heat deformation temperature / ℃ 0-1 F401 without nucleating agent 32.72 1293.515 98.9 2-1 Test Example 2 79.74 1374.24 102.8 2-2 Test Example 2 83.31 1311.48 103.6 2-3 Test Example 2 82.62 1335.08 105.7 2-4 Test Example 2 74.88 1409.35 102.3 2-5 Test Example 2 73.66 1486.42 103.2 2-6 Test Example 2 71.34 1459.63 102.9

[0060] Table 3 Results of different rigidity-toughness balance nucleating agents for modified copolymerized polypropylene PPB240 (addition amount 0.1%)

[0061] Serial number Impact strength J / m Flexural modulus / MPa Heat deformation temperature / ℃ 0-2 PPB240 without nucleating agent 626.33 1309.67 75.1 3-1 Test Example 3 815.65 1336.28 76.5 3-2 Test Example 3 857.3 1333.41 81.4 3-3 Test Example 3 864.99 1343.72 85.1 3-4 Test Example 3 888.62 1324.79 72.8 3-5 Test Example 3 909.67 1310.14 75.7 3-6 Test Example 3 884.51 1328.50 76.3

[0062] Compared with 0-2 to 3-6, the rigidity-toughness balanced nucleating agent can also effectively improve the impact performance, flexural modulus and heat deformation temperature of PPB240.

[0063] Table 4 Results of different rigidity-toughness balance nucleating agents for modified copolymerized polypropylene PPB240 (addition amount 0.2%)

[0064] Serial number Impact strength KJ / m2 Flexural modulus / MPa Heat deformation temperature / ℃ 0-2 PPB240 without nucleating agent 626.33 1309.67 75.1 4-1 Test Example 4 836.88 1332.41 79.5 4-2 Test Example 4 874.84 1319.42 83.02 4-3 Test Example 4 889.11 1330.23 88.90 4-4 Test Example 4 907.91 1326.77 79.52 4-5 Test Example 4 918.82 1341.52 78.39 4-6 Test Example 4 909.52 1333.08 79.86

[0065] Table 5: Comparative Examples 1-4 Results

[0066] Serial number Impact strength KJ / m2 Flexural modulus / MPa Heat deformation temperature / ℃ 0-1 F401 without nucleating agent 32.72 1293.515 98.9 5-1 Comparative Example 1 58.83 1281.63 92.6 5-2 Comparative Example 2 64.51 1290.26 94.1 0-2 PPB240 without nucleating agent 626.33 1309.67 75.1 6-1 Comparative Example 3 678.29 1398.27 87.5 6-2 Comparative Example 4 606.93 1390.74 89.3

[0067] Comparing the data in Table 5 with Tables 1-4, under the addition ratio of the comparative example, adding toughening and stiffening nucleating agents will only improve toughness or stiffness, while adding a stiffness-toughness balance nucleating agent will improve both stiffness and toughness of the polypropylene product.

[0068] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a rigid-tough balanced nucleating agent, characterized in that: Specifically, the method comprises the following steps: adding nadic anhydride to an ester solvent to obtain a mixed solution, dropping an amine substance into the mixed solution, reacting at 40 to 60° C. to obtain an amic acid precipitate, filtering, washing, and drying the amic acid precipitate; using water as a solvent, reacting the obtained amic acid with a first main group metal oxide under heating conditions of 60 to 80° C. to obtain a rigid-tough balanced nucleating agent; The molar ratio of the nadic anhydride to the amine substance is 1:1 to 1:1.5; the molar ratio of the amic acid to the first main group metal oxide is 1:0.2 to 1:1; the amount of the solvent water added is 2 to 5 times the mass of the amic acid precipitate; The amine substance is one of benzylidene amine and dodecylamine; 2. The method for preparing a rigid-tough balanced nucleating agent according to claim 1, characterized in that: The first main group metal oxide is one of lithium oxide, sodium oxide and potassium oxide.

3. The method for preparing a rigid-tough balanced nucleating agent according to claim 1, characterized in that: The ester solvent is ethyl acetate, and the concentration of nadic anhydride in the ethyl acetate solvent is 5-15 mol / L.

4. The method for preparing a rigid-tough balanced nucleating agent according to claim 1, characterized in that: The molar ratio of the amic acid to the first main group metal oxide is 1:0.

5.

5. The method for preparing a rigid-tough balanced nucleating agent according to claim 1, characterized in that: The amount of solvent water added is 4 times the mass of the amic acid precipitate.

6. A rigid-tough balanced nucleating agent prepared by the method according to any one of claims 1 to 5.

7. The rigid-tough balanced nucleating agent according to claim 6, characterized in that: The rigid-tough balanced nucleating agent is any one of bicyclo[2.2.1]heptene-2-benzylamide-3-carboxylate lithium, bicyclo[2.2.1]heptene-2-benzylamide-3-carboxylate sodium, bicyclo[2.2.1]heptene-2-benzylamide-3-carboxylate potassium, bicyclo[2.2.1]heptene-2-dodecylamide-3-carboxylate lithium, bicyclo[2.2.1]heptene-2-dodecylamide-3-carboxylate sodium, and bicyclo[2.2.1]heptene-2-dodecylamide-3-carboxylate potassium.

8. Use of the rigidity-toughness balanced nucleating agent according to claim 6 or 7 in polypropylene to improve the impact strength, flexural modulus and heat deformation temperature of polypropylene.

9. The use of the rigid-tough balanced nucleating agent in polypropylene according to claim 8, characterized in that: The rigid-tough balanced nucleating agent is added to polypropylene at a concentration of 0.1 wt% to 0.3 wt%.

10. The use of the rigid-toughness balanced nucleating agent in polypropylene according to claim 9, characterized in that: The polypropylene is added with an antioxidant, an acid absorbent and the nucleating agent, mixed and stirred evenly in a high-speed mixer, and then extruded and granulated by a twin-screw extruder.