Liquid crystal / polymer composite material, preparation method thereof, dimming film containing liquid crystal / polymer composite material and application of dimming film

By designing liquid crystal/polymer composite materials with high infrared emissivity, the problem that liquid crystal/polymer composite materials in the prior art do not have radiation refrigeration function is solved, and high-efficiency radiation refrigeration effect within the range of 20-70℃ is achieved. And improves the energy-saving potential of buildings and cars.

CN118878734AActive Publication Date: 2024-11-01PEKING UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411266430.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-19
Filing Date
2024-09-10
Publication Date
2024-11-01
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

Existing liquid crystal/polymer composite materials do not have effective radiation refrigeration functions and cannot effectively reduce energy consumption and temperature of buildings and cars.

Method used

A liquid crystal/polymer composite material is designed, including a polymer network skeleton and liquid crystal molecules dispersed therein, through a specific structural design, so that it has an 8-13 μm atmospheric window of more than 90% in the range of 20-70°C. Infrared emissivity, combined with the preparation method and the application of dimming film, achieves the radiation refrigeration effect.

Benefits of technology

It realizes efficient radiation refrigeration in the range of 20-70℃, enhances the potential of energy-saving and thermal insulation, has good mechanical strength and is suitable for large-scale manufacturing, and can produce large-area flexible films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878734A_ABST
    Figure CN118878734A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of functional liquid crystal materials, and discloses a liquid crystal / polymer composite material, a preparation method thereof, a dimming film and application. The composite material comprises a macromolecular network skeleton and liquid crystal molecules dispersed in the macromolecular network skeleton, wherein the liquid crystal molecule has a structure as shown in a formula I. Mixing liquid crystal molecules, a polymerizable monomer, an initiator and spacer particles to obtain a prepolymer; and curing the obtained prepolymer through heating or illumination to obtain the liquid crystal / polymer composite material. The invention further provides a dimming film containing the composite material and application of the dimming film to energy conservation of automobiles and buildings. Compared with the prior art, the liquid crystal / polymer composite material provided by the invention has higher refrigeration power at the same temperature, and has higher potential in energy conservation, heat preservation and temperature control; the film has good mechanical strength and large-scale manufacturing capability, and can be used for manufacturing large-area flexible films.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-references

[0002] This application claims priority to the Chinese patent application filed on April 19, 2024, with application number 202410471763.8, and invention name “Liquid crystal / polymer composite materials and preparation methods thereof, dimming films containing the same and applications”, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present invention relates to the technical field of functional liquid crystal materials, and in particular to a liquid crystal / polymer composite material and a preparation method thereof, a dimming film containing the same, and applications thereof. Background Art

[0004] With the overuse of fossil fuels, mankind is facing a serious crisis of energy shortage and global warming, which threatens the sustainable development of human society. From a global perspective, buildings consume 40% of the world's energy, and windows are one of the least energy-efficient parts, accounting for about 60% of the energy consumption and loss of buildings.

[0005] Thermal radiation is fundamentally generated from the random energy level transitions of matter, indicating that any object at a finite temperature can intrinsically achieve thermal emission of energy. The universe has a temperature close to absolute zero, and objects on Earth can dissipate heat into outer space in the form of electromagnetic waves, achieving radiation cooling. Radiative cooling achieves cooling without any additional input energy. The atmosphere in the space between the Earth's surface and the universe is a complex mixture of various gases. The low transmittance of the atmosphere itself makes the Earth's surface have a weakening effect on cosmic thermal radiation in most bands. Only within the atmospheric window range of 8-13μm is the atmosphere highly transparent to thermal radiation. This atmospheric window coincides with the peak wavelength of thermal radiation from Earth objects at typical ambient temperatures (around 25°C). Therefore, any ground object with high emissivity within the atmospheric window can reduce its own temperature by radiating heat into outer space.

[0006] Liquid crystal / polymer composite materials are one of the most promising building energy-saving materials. By giving liquid crystal / polymer composite materials the function of radiation cooling, the energy-saving effect of liquid crystal / polymer materials can be further enhanced, which has important practical significance for achieving efficient energy saving in automobiles and buildings. The original liquid crystal / polymer composite materials are not conducive to radiation cooling.

[0007] Therefore, there is an urgent need to develop a liquid crystal / polymer composite material with radiative cooling function. Summary of the invention

[0008] The purpose of the present invention is to overcome the problems existing in the prior art and to provide a liquid crystal / polymer composite material with stable radiation cooling function, a dimming film containing the same, and a preparation method and application thereof.

[0009] The total infrared emissivity of the liquid crystal / polymer composite material provided by the present invention in the atmospheric window at an ambient temperature of 20-70° C. is not less than 90%, and therefore has a radiation cooling effect.

[0010] In order to achieve the above-mentioned object, the first aspect of the present invention provides a liquid crystal / polymer composite material, wherein the composite material comprises a polymer network skeleton and liquid crystal molecules dispersed inside the polymer network skeleton;

[0011] Wherein, the liquid crystal molecule has a structure described in Formula I:

[0012]

[0013] Wherein, R1 is selected from C1-C 16 Alkyl, C1-C 16 Alkoxy or C1-C 16 Siloxane group;

[0014] Y and Z are each independently selected from an ester bond, a C1-C4 alkylene bond, an ether bond or a single bond;

[0015] Ring X is independently selected from the following structures:

[0016]

[0017] When the number of ring X in formula I is two or more, the rings of each structure are connected to each other through a C1-C4 alkylene bond, an ether bond, an ester bond or a single bond;

[0018] R2 is selected from one of the following structures:

[0019]

[0020] m is a positive integer of 1-8; n is a positive integer of 0-16.

[0021] A second aspect of the present invention provides a method for preparing the composite material according to the first aspect, wherein the method comprises the following steps:

[0022] (1) mixing liquid crystal molecules, polymerizable monomers, initiators and spacer particles to obtain a prepolymer;

[0023] (2) Curing the prepolymer obtained in step (1) by heating or irradiation with light to obtain a liquid crystal / polymer composite material.

[0024] The third aspect of the present invention provides a dimming film comprising the composite material described in the first aspect or the composite material obtained by the preparation method of the second aspect. The liquid crystal / polymer composite material provided by the present invention can achieve reversible switching between a light scattering state and a transparent state under the control of an electric field or temperature, and can be used as a dimming film, while having a radiation cooling effect.

[0025] The fourth aspect of the present invention provides the use of the liquid crystal / polymer composite material according to the first aspect or the dimming film according to the third aspect in energy saving for automobiles and buildings.

[0026] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:

[0027] (1) The liquid crystal / polymer composite material provided by the present invention has an infrared emissivity of more than 90% of the 8-13 μm atmospheric window within the temperature range of 20-70°C, and has stable radiation cooling capability;

[0028] (2) Compared with the prior art, the liquid crystal / polymer composite material provided by the present invention has a greater cooling power at the same temperature and has greater potential in energy saving, heat preservation and temperature control; it has good mechanical strength and the ability to be mass-produced, and can be used to manufacture large-area flexible films. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 is a morphology diagram of the polymer network skeleton in the dimming film prepared in Example 1 of the present invention;

[0030] Figure 2 is a morphology diagram of the polymer network skeleton in the dimming film prepared in Example 2 of the present invention;

[0031] Figure 3 is the near-infrared absorption spectrum of the liquid crystal molecules used in Example 1 of the present invention;

[0032] Figure 4 is the near-infrared absorption spectrum of the liquid crystal molecules used in Comparative Example 1 of the present invention;

[0033] Figure 5 is the ultraviolet, visible and near infrared light transmittance of the dimming film prepared in Example 1 of the present invention;

[0034] Figure 6 is the infrared light emissivity curve of 8-13 μm of the dimming film prepared in Example 1 of the present invention;

[0035] Figure 7 is the infrared light emissivity curve of 8-13 μm of the dimming film prepared in Example 2 of the present invention;

[0036] Figure 8is the infrared light emissivity curve of 8-13 μm of the dimming film prepared in Example 3 of the present invention;

[0037] Fig. 9 is the infrared light emissivity curve of 8-13 μm of the dimming film prepared in Example 4 of the present invention;

[0038] Fig.10 is the infrared light emissivity curve of 8-13 μm of the dimming film prepared in Comparative Example 1 of the present invention;

[0039] Fig.11 is the infrared light emissivity curve of 8-13 μm of the dimming film prepared in Comparative Example 2 of the present invention;

[0040] Fig.12 is the light transmittance of the dimming film prepared in Example 2 of the present invention when an electric field is applied and when no electric field is applied;

[0041] Fig.13 is the light transmittance of the dimming film prepared in Example 3 of the present invention when no electric field is applied and when a 100V 50Hz AC electric field is applied;

[0042] Fig.14 The embodiment 1 of the present invention and the PET film at 800W / m 2 Temperature change comparison curve under sunlight simulation conditions. DETAILED DESCRIPTION

[0043] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0044] The first aspect of the present invention provides a liquid crystal / polymer composite material, wherein the composite material comprises a polymer network skeleton and liquid crystal molecules dispersed inside the polymer network skeleton;

[0045] Wherein, the liquid crystal molecule has a structure described in Formula I:

[0046]

[0047] Wherein, R1 is selected from C1-C 16 Alkyl, C1-C 16 Alkoxy or C1-C 16 Siloxane group;

[0048] Y and Z are each independently selected from an ester bond, a C1-C4 alkylene bond, an ether bond or a single bond;

[0049] Ring X is independently selected from the following structures:

[0050]

[0051] When the number of ring X in formula I is two or more, the rings of each structure are connected to each other through a C1-C4 alkylene bond, an ether bond, an ester bond or a single bond;

[0052] R2 is selected from one of the following structures:

[0053]

[0054] m is a positive integer of 1-8; n is a positive integer of 0-16.

[0055] Among them, C1-C 16 Alkyl refers to an alkyl group containing 1-16 carbon atoms, and the number of carbon atoms can be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16;

[0056] C1-C 16 Alkoxy refers to an alkoxy group containing 1-16 carbon atoms, and the number of carbon atoms can be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16;

[0057] C1-C 16 The siloxane group refers to a siloxane group containing 1-16 carbon atoms, and the number of carbon atoms can be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, or 16.

[0058] The value of m can be 1, 2, 3, 4, 5, 6, 7, 8; the value of n can be 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16. Preferably, m is a positive integer of 2-8.

[0059] In Formula I, ring X is a ring structure, such as a six-membered ring, a condensed ring, etc. m refers to the total number of X (liquid crystal rigid structure). Please note that the structure shown in Formula I is a liquid crystal molecule, which is not a polymer compound (relative molecular weight can reach 10 4 -10 7 ), m is not the degree of polymerization (the number of repeating structural units).

[0060] For example, when m is 2, there are two rings; the two groups represented by the two rings may be the same or different. When the two rings are the same group or different groups, they may be connected by a C1-C4 alkylene group, an ether bond, an ester bond or a single bond. The groups refer to the various cyclic structures (types of ring X) listed above.

[0061] The present invention creatively designs the structure of liquid crystal molecules so that the liquid crystal / polymer composite material containing liquid crystal molecules has improved radiation cooling properties, and the infrared emissivity in the atmospheric window (8-13 μm) at 20-70° C. is greater than 90%. The liquid crystal molecules are rod-shaped thermotropic liquid crystals whose liquid crystal phase temperature range covers room temperature. In practical applications, a variety of liquid crystal molecules falling into formula I are usually selected and mixed as raw materials for preparing liquid crystal / polymer composite materials.

[0062] In some embodiments of the present invention, the liquid crystal molecules are selected from at least one of a first component, a second component and a third component;

[0063] Wherein, the first component is selected from at least one of the compound of formula (1-a) and the compound of formula (1-b):

[0064]

[0065] Wherein, Ra is a C3-C7 alkyl group; Rb is a C2-C6 alkyl group;

[0066] R is selected from one of the following structures:

[0067]

[0068] The second component is selected from at least one of the compounds of formula (2-c):

[0069]

[0070] Wherein, Rc is a C2-C4 alkyl group; Rd is a C3-C5 alkyl group;

[0071] The third component is selected from at least one of the compounds of formula (3-d):

[0072]

[0073] Wherein, Re is the group represented by R1-Y; Rf is the group represented by R2-Z.

[0074] Among them, C3-C7 alkyl refers to an alkyl group containing 3-7 carbon atoms, and the number of carbon atoms can be 3, 4, 5, 6, or 7; C2-C6 alkyl refers to an alkyl group containing 2-6 carbon atoms, and the number of carbon atoms can be 2, 3, 4, 5, or 6;

[0075] C2-C4 alkyl refers to an alkyl group containing 2-4 carbon atoms, and the number of carbon atoms can be 2, 3, or 4;

[0076] C3-C5 alkyl refers to an alkyl group containing 3-5 carbon atoms, and the number of carbon atoms can be 3, 4, or 5.

[0077] Each compound of the first component, the second component and the third component mentioned above falls within the scope of Formula I. For example, when phenylene and cyclohexylene (connected by a single bond) are selected, m is 2, and Formula (1-b) can be obtained.

[0078] In some embodiments of the present invention, the liquid crystal molecules include, by weight percentage: 25-60% of the first component, 5-30% of the second component and 20-45% of the third component. In the present invention, the liquid crystal molecules are stable and will not produce the adverse effect of phase separation caused by long-term placement. In addition, the birefringence is greater, and the contrast of the corresponding temperature-controlled and electrically-controlled composite is higher.

[0079] In some embodiments of the present invention, the liquid crystal molecules are selected from at least one of the following structures:

[0080]

[0081] In some embodiments of the present invention, the liquid crystal molecules include the above six components, and their weight percentages are 26%, 13%, 12%, 6%, 40%, and 3%, respectively. In some embodiments of the present invention, the liquid crystal molecules are selected from at least one of trans, trans-4'-propyl-4-(3,4,5-trifluorophenyl)bicyclohexane, 5-4-(3,4-difluorophenyl)-4'-propyl-1,1'-bis(cyclohexane), (trans, trans)-4-ethyl-4'-propylbicyclohexylane and (trans, trans)-4-propyl-4'-butyl-1,1'-bicyclohexane.

[0082] In some embodiments of the present invention, the liquid crystal molecules include, by weight percentage: 18.75% (trans, trans)-4-ethyl-4'-propylbis(cyclohexyl)ethane, 50% 5-4-(3,4-difluorophenyl)-4'-propyl-1,1'-bis(cyclohexane), 25% trans, trans-4'-propyl-4-(3,4,5-trifluorophenyl)bis(cyclohexane)ethane and 6.25% (trans, trans)-4-propyl-4'-butyl-1,1'-bicyclohexane.

[0083] The structural formula of trans, trans-4'-propyl-4-(3,4,5-trifluorophenyl)bicyclohexane is:

[0084]

[0085] The structural formula of 5-4-(3,4-difluorophenyl)-4'-propyl-1,1'-bis(cyclohexane) is:

[0086]

[0087] The structural formula of (trans, trans)-4-ethyl-4'-propylbicyclohexyl alkane is:

[0088]

[0089] The structural formula of (trans, trans)-4-propyl-4'-butyl-1,1'-bicyclohexane is:

[0090]

[0091] In some embodiments of the present invention, the liquid crystal molecules are selected from at least one of ethylcyclohexylphenyl-2,3-difluorophenethyl ether, ethylcyclohexyl-2,3-difluorophenethyl ether, propyldicyclohexyl-2,3-difluoromethylbenzene, propylcyclohexyl-2,3-difluorophenylbutyl ether and propylcyclohexyl-2,3-difluorophenethyl ether.

[0092] In some embodiments of the present invention, the liquid crystal molecules include the above five components, and the weight percentages thereof are 53.8%, 23.1%, 8.5%, 7.7% and 6.9%, respectively.

[0093] In some embodiments of the present invention, the polymer network skeleton is selected from at least one of a polymer dispersed liquid crystal (PDLC) structure, a polymer stabilized liquid crystal (PSLC) structure, and a composite structure (PD&SLC) composed of the two.

[0094] In some embodiments of the present invention, the polymer network skeleton is polymerized by heating or irradiating a polymerizable monomer having a mid-infrared emission function, wherein the polymerizable monomer contains halogen, saturated aliphatic hydrocarbon, ether bond, silicon-oxygen bond, and the like.

[0095] In some embodiments of the present invention, the polymerizable monomers include polymerizable monomers mainly based on flexible alkyl chains (generally non-liquid crystal) and rigid polymerizable monomers with shape anisotropy (generally liquid crystal, but not absolutely).

[0096] A second aspect of the present invention provides a method for preparing the composite material according to the first aspect, wherein the method comprises the following steps:

[0097] (1) mixing liquid crystal molecules, polymerizable monomers, initiators and spacer particles to obtain a prepolymer;

[0098] (2) Curing the prepolymer obtained in step (1) by heating or irradiation with light to obtain a liquid crystal / polymer composite material.

[0099] In step (2), the prepolymer can be first sandwiched between two layers of transparent conductive glass or conductive ITO film, and the thickness of the prepolymer liquid is controlled to be 5-50 μm. The prepolymer is then cured by heating (thermal polymerization monomer) or light (free radical or cationic photopolymerization monomer) to obtain a liquid crystal / polymer composite material with a PDLC structure.

[0100] In some embodiments of the present invention, the liquid crystal molecules in step (1) include chiral compounds; step (2) further includes: vertically aligning the liquid crystal molecules by means of a vertical alignment agent or applying a low-frequency alternating electric field, and then curing the prepolymer by heating (thermal polymerization monomer) or light irradiation (free radical or cationic photopolymerization monomer) to obtain a liquid crystal / polymer composite material with a PSLC structure; or,

[0101] After the prepolymer is cured to obtain the PDLC structure, an electric field is applied to vertically align the liquid crystal molecules, and a second heating or light irradiation is performed to induce free radical or cationic polymerization of the monomers to obtain a liquid crystal / polymer composite material with a PD&SLC structure.

[0102] In step (1), the proportions of the raw materials may be: liquid crystal molecules: 10-80 parts by weight; polymerizable monomers: 10-80 parts by weight; initiators: 0.1-5 parts by weight; and spacer particles: 0.1-2 parts by weight. The spacer particles may be silicon dioxide.

[0103] The liquid crystal / polymer composite material prepared by the invention has an emissivity higher than 90% in an atmospheric window at 20-70° C. and has a stable radiation cooling function.

[0104] The third aspect of the present invention provides a dimming film comprising the composite material described in the first aspect or the composite material obtained according to the preparation method described in the second aspect. For example, the dimming film comprises two layers of transparent conductive glass or conductive ITO film and the liquid crystal / polymer composite material provided by the present invention sandwiched therebetween.

[0105] The fourth aspect of the present invention provides the use of the liquid crystal / polymer composite material according to the first aspect or the dimming film according to the third aspect in energy saving for automobiles and buildings.

[0106] The present invention will be described in detail below through examples.

[0107] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be obtained through commercial channels.

[0108] In the following examples and comparative examples, the polymerizable monomers in Examples 1-2 and Comparative Example 1 are: 58.2 wt % of isobornyl acrylate IBOA 18.2 wt% 1,4-Butanediol diacrylate BDDA 14.5 wt% 3-(trimethoxysilyl)propyl methacrylate TMSPMA and 9.1wt% C6M

[0109]

[0110] The initiator is the photoinitiator Irg651 (2,2-dimethoxy-1,2-diphenylethan-1-one,

[0111] Spacer particles: purchased from Sekisui Chemical Co., Ltd.

[0112] Example 1

[0113] This example is used to illustrate the preparation of a dimming film comprising a liquid crystal / polymer composite material having a radiation cooling function.

[0114] In this embodiment, the liquid crystal molecules include the components in Table 1 (purchased from Yantai Xianhua Technology Group Co., Ltd.):

[0115] Table 1

[0116]

[0117]

[0118]

[0119] in, References: Abhilash TK, Varghese H, Czerwiński M, et al. Probing the effect of chiral dopantfluorination on dielectric and electro-optical properties of the ferroelectric liquid crystalline mixture [J]. Journal of Molecular Liquids, 2021, 341: 117392.

[0120] (1) 77% of liquid crystal molecules, 22% of polymerizable monomers, 0.5% of initiators and 0.5% of spacer particles (average particle size of 20 μm) were mixed and stirred at room temperature to form an isotropic mixed solution; then, the mixed solution was ultrasonicated for 15 minutes; the total mass of the mixed solution was 20 g;

[0121] (2) coating the obtained mixed solution between two plastic films coated with indium tin oxide (ITO) transparent conductive films, and rolling them evenly to form a thin film; irradiating the thin film with 365nm ultraviolet light at room temperature with an intensity of 1mw / cm 2 , the illumination time is 60s; then the film is made into an upper electrode, a 10Hz, 100V square wave alternating current is applied, and it is continuously irradiated with 365nm ultraviolet light for 10min to form a temperature-controlled dimming film with a PD&SLC structure.

[0122] Example 2

[0123] This example is used to illustrate the preparation of a dimming film comprising a liquid crystal / polymer composite material having a radiation cooling function.

[0124] In this embodiment, the liquid crystal molecules include 18.75% of (trans, trans)-4-ethyl-4'-propylbis(cyclohexyl)ethane, 50% of 5-4-(3,4-difluorophenyl)-4'-propyl-1,1'-bis(cyclohexane), 25% of trans, trans-4'-propyl-4-(3,4,5-trifluorophenyl)bis(cyclohexane)ethane and 6.25% of (trans, trans)-4-propyl-4'-butyl-1,1'-dicyclohexane, all of which were purchased from Yantai Xianhua Technology Group Co., Ltd.

[0125] (1) 77% of liquid crystal molecules, 22% of polymerizable monomers, 0.5% of initiators and 0.5% of spacer particles (average particle size of 50 μm) were mixed and stirred at room temperature to form an isotropic mixed solution; then, the mixed solution was ultrasonicated for 15 minutes; the total mass of the mixed solution was 20 g;

[0126] (2) coating the obtained mixed solution between two plastic films coated with indium tin oxide (ITO) transparent conductive films to form a film; irradiating the film with 365nm ultraviolet light at room temperature with an intensity of 5mw / cm 2 The illumination time is 600s, and an electric field responsive dimming film with a PDLC structure is manufactured.

[0127] Because the PDLC structure does not require electrical polymerization during polymerization, the thickness can be greater than the liquid crystal / polymer composite of the temperature-controlled PDLC and PSLC structure coexistence system. Thickness and temperature will affect the transmittance and emissivity in the off state.

[0128] Example 3

[0129] This example is used to illustrate the preparation of a dimming film comprising a liquid crystal / polymer composite material having a radiation cooling function.

[0130] In this embodiment, negative liquid crystal monomers were purchased from Beijing Bayi Space-Time Liquid Crystal Technology Co., Ltd.: 323178-01-4, ethylcyclohexylphenyl-2,3-difluorophenyl ether; 415915-41-2, ethylcyclohexyl-2,3-difluorophenyl ether; 174350-06-2, propyldicyclohexyl-2,3-difluoromethylbenzene; 208709-55-1, propylcyclohexyl-2,3-difluorophenyl butyl ether; 174350-05-1, propylcyclohexyl-2,3-difluorophenyl ether; weight ratios were 53.8%, 23.1%, 8.5%, 7.7%, and 6.9%. The liquid crystal mixture composed of the above liquid crystal monomers was used as the liquid crystal molecules of this embodiment.

[0131] Table 2

[0132]

[0133]

[0134] (1) 94% of liquid crystal molecules, 5% of polymerizable monomers (C6M), 0.5% of initiators and 0.5% of spacer particles (average particle size of 20 μm) were mixed and stirred at room temperature to form an isotropic mixed solution; then, the mixed solution was ultrasonicated for 15 minutes; the total mass of the mixed solution was 20 g;

[0135] (2) Using the capillary principle, the obtained mixed solution was poured into a 20 μm 4 cm × 5 cm commercial vertical alignment liquid crystal empty box (the commercial liquid crystal box is composed of two layers of SiO2 glass coated with ITO, with glass beads in the middle to control the thickness) using a capillary tube; the filled liquid crystal box was placed on a microscope hot stage set at 50°C and irradiated with 365 nm ultraviolet light with an intensity of 10 mw / cm 2 , the illumination time is 300 s, and an electric field responsive dimming film with a PSLC structure is manufactured.

[0136] Example 4

[0137] This example is used to illustrate the preparation of a dimming film comprising a liquid crystal / polymer composite material having a radiation cooling function.

[0138] In this embodiment, the liquid crystal molecules are the same as those in the first embodiment.

[0139] (1) 94% of liquid crystal molecules, 5% of polymerizable monomers (C6M), 0.5% of initiators and 0.5% of spacer particles (average particle size of 20 μm) were mixed and stirred at room temperature to form an isotropic mixed solution; then, the mixed solution was ultrasonicated for 15 minutes; the total mass of the mixed solution was 20 g;

[0140] (2) Using the capillary principle, the obtained mixed solution was poured into a 20 μm 4 cm × 5 cm commercial vertical alignment liquid crystal empty box using a capillary tube; at room temperature, it was irradiated with 365 nm ultraviolet light with an intensity of 10 mW / cm 2 The illumination time is 300s, and a temperature-responsive dimming film with a PSLC structure is prepared.

[0141] Comparative Example 1

[0142] The dimming film was prepared according to the method of Example 1, except that the liquid crystal molecules were 30 wt % of nematic liquid crystal E8 and 70 wt % of smectic liquid crystal 8CB (4′-octyl-4-biphenylcarbonitrile), both purchased from Yantai Xianhua Technology Group Co., Ltd.

[0143] Comparative Example 2

[0144] The dimming film was prepared according to the method of Example 2, except that all the liquid crystal molecules were nematic liquid crystal E8 purchased from Yantai Xianhua Technology Group Co., Ltd.

[0145] Test Example 1

[0146] The morphology of the polymer network in the dimming film prepared in Example 1 and Example 2 was studied using a scanning electron microscope (SEM, JSM-6700F). To examine the polymer network, the film was first immersed in cyclohexane at room temperature for one week to remove the liquid crystal molecules, and a gold coating was sprayed on the film to remove any charge. The polymer network structure of the liquid crystal / polymer composite material is shown in FIG. Figure 1 , Figure 2 shown.

[0147] Figure 1 The PD&SLC vertical cross-section porous structure has pores that are oriented in the vertical direction, which makes the liquid crystal rod-shaped molecules in the network tend to be arranged vertically. When the liquid crystal molecules are in the smectic phase, the molecules are arranged vertically and transmit sunlight. The liquid crystal in the cholesteric phase tends to be arranged in a spiral, which will interact with the vertical polymer network to form a focal conic arrangement conformation and scatter sunlight.

[0148] Figure 2It is a standard porous structure of PDLC, and the size of the pores is about 10μm. The cross-linking reaction of the polymer monomer is induced by ultraviolet light irradiation or heating. As the molecular chain of the polymer monomer continues to grow, the solubility of the small molecule liquid crystal material in the polymer continues to decrease, so that it precipitates, merges and grows in the form of liquid crystal droplets. When the polymerization is complete, the liquid crystal droplets are uniformly dispersed in the polymer matrix of the continuous phase in the form of a discontinuous phase, and the porous structure of the PDLC membrane is obtained.

[0149] Test Example 2

[0150] The near infrared absorption spectra of the liquid crystal molecules used in Example 1 and Comparative Example 1 are as follows: Figure 3 and Figure 4 shown.

[0151] E8 in Comparative Example 1 is a liquid crystal molecule containing a cyano group. Figure 4 Medium, from 2220-2230cm -1 The strong absorption peak of cyano can be seen at 1500-600cm -1 ), which causes it to absorb excess infrared light, reduce its selective emissivity in the atmospheric window (8-13μm), and ultimately reduce the radiative cooling efficiency of the composite material.

[0152] and Figure 3 There is no cyanide peak in it, it is a fluorine-containing liquid crystal, and the infrared absorption peak is at 1500-600cm -1 .

[0153] Test Example 3

[0154] The UV-visible-near infrared light transmittance of the dimming film prepared in Example 1 was tested at room temperature (25° C.) and 45° C. using a variable temperature UV-visible-near infrared spectrophotometer. Figure 5 As shown, the test wavelength is 300-2500 nm, which proves that the liquid crystal / polymer composite of Example 1 can achieve the change of transmittance in the sunlight band.

[0155] Test Example 4

[0156] The infrared light emissivity curves of 8-14 μm of the dimming films prepared in Examples 1-4 and Comparative Examples 1 and 2 were measured using a Fourier transform infrared spectrometer equipped with a gold integrating sphere (ISR-603). Figure 6-11 shown.

[0157] from Fig.10 It can be seen that the emissivity of the dimming film prepared in Comparative Example 1 is around 90%, while the emissivity of the dimming film prepared in Example 1 is around 95% (eg Figure 6 shown).

[0158] from Fig.11 It can be seen that the emissivity of the dimming film prepared in Comparative Example 2 is below 85%, while the emissivity of the dimming film prepared in Example 2 is above 90%.

[0159] Test Example 5

[0160] The light transmittance of the dimming film prepared in Example 2 when an electric field is applied and when no electric field is applied is tested using a transformer and a UV-visible-near infrared spectrophotometer. Fig.12 As shown, the test wavelength is 500-2500nm.

[0161] The light transmittance of the dimming film prepared in Example 3 when no electric field was applied and when a 100V 50Hz AC electric field was applied was tested using a variable temperature UV-Vis-NIR spectrophotometer. Fig.13 As shown, the test wavelength is 300-2500nm.

[0162] Fig.12 and 13 It is explained that the dimming film prepared by the present invention can realize precise control of temperature. On the premise that the material itself has high radiation cooling power brought by high emissivity, the input power of sunlight can be affected by controlling the transmittance, thereby affecting the final total cooling power.

[0163] Test Example 6

[0164] In a laboratory with a constant temperature of 25°C, the PET film and the dimming film of Example 1 with the same initial temperature were heated at 800 W / m 2 The samples were then placed under the sunlight simulating lamp for three minutes until the temperatures of the two materials stabilized. Fig.14 As shown, when the temperatures of the two materials are stable, the difference in stable temperature is about 13.5° C., which indicates that Example 1 achieves a higher total radiation cooling effect than the PET film.

[0165] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A liquid crystal / polymer composite material, characterized in that: The composite material comprises a polymer network skeleton and liquid crystal molecules dispersed inside the polymer network skeleton; Wherein, the liquid crystal molecule has a structure described in Formula I: Wherein, R1 is selected from C1-C 16 Alkyl, C1-C 16 Alkoxy or C1-C 16 Siloxane group; Y and Z are each independently selected from an ester bond, a C1-C4 alkylene bond, an ether bond or a single bond; Ring X is independently selected from the following structures: When the number of ring X in formula I is two or more, the rings of each structure are connected to each other through a C1-C4 alkylene bond, an ether bond, an ester bond or a single bond; R2 is selected from one of the following structures: m is a positive integer of 1-8; n is a positive integer of 0-16.

2. The composite material according to claim 1, wherein m is a positive integer from 2 to 8; Preferably, the liquid crystal molecules are selected from at least one of a first component, a second component and a third component; wherein the first component is selected from at least one of a compound of formula (1-a) and a compound of formula (1-b): Wherein, Ra is a C3-C7 alkyl group; Rb is a C2-C6 alkyl group; R is selected from one of the following structures: The second component is selected from at least one of the compounds of formula (2-c): Wherein, Rc is a C2-C4 alkyl group; Rd is a C3-C5 alkyl group; The third component is selected from at least one of the compounds of formula (3-d): Wherein, Re is the group indicated by R1-Y in claim 1; Rf is the group indicated by R2-Z in claim 1; Preferably, the liquid crystal molecules include, by weight percentage: 25-60% of the first component, 5-30% of the second component and 20-45% of the third component.

3. The composite material according to claim 1, wherein The liquid crystal molecules are selected from at least one of the following structures: Preferably, the liquid crystal molecules include the above six components, and the weight percentages thereof are 26%, 13%, 12%, 6%, 40% and 3%, respectively.

4. The composite material according to claim 1, wherein The liquid crystal molecules are selected from at least one of trans, trans-4'-propyl-4-(3,4,5-trifluorophenyl)bicyclohexane, 5-4-(3,4-difluorophenyl)-4'-propyl-1,1'-bis(cyclohexane), (trans, trans)-4-ethyl-4'-propylbicyclohexane and (trans, trans)-4-propyl-4'-butyl-1,1'-bicyclohexane; Preferably, the liquid crystal molecules include, by weight percentage: 18.75% of (trans, trans)-4-ethyl-4'-propylbis(cyclohexyl)ethane, 50% of 5-4-(3,4-difluorophenyl)-4'-propyl-1,1'-bis(cyclohexane), 25% of trans, trans-4'-propyl-4-(3,4,5-trifluorophenyl)bis(cyclohexane)ethane and 6.25% of (trans, trans)-4-propyl-4'-butyl-1,1'-bicyclohexane.

5. The composite material according to claim 1, wherein The liquid crystal molecules are selected from at least one of ethylcyclohexylphenyl-2,3-difluorophenyl ether, ethylcyclohexyl-2,3-difluorophenyl ether, propyldicyclohexyl-2,3-difluoromethylbenzene, propylcyclohexyl-2,3-difluorophenyl butyl ether and propylcyclohexyl-2,3-difluorophenyl ether; Preferably, the liquid crystal molecules include the above five components, and the weight percentages thereof are 53.8%, 23.1%, 8.5%, 7.7% and 6.9% respectively.

6. The composite material according to claim 1, wherein The polymer network skeleton is selected from at least one of a polymer dispersed liquid crystal structure, a polymer stabilized liquid crystal structure, and a composite structure composed of the two; And / or, the polymer network skeleton is polymerized by polymerizable monomers having mid-infrared emission function under heating or light; And / or, the polymerizable monomers include polymerizable monomers mainly composed of flexible alkyl chains and rigid polymerizable monomers with anisotropic shapes.

7. A method for preparing a composite material according to claim 1, characterized in that: The method comprises the following steps: (1) mixing liquid crystal molecules, polymerizable monomers, initiators and spacer particles to obtain a prepolymer; (2) Curing the prepolymer obtained in step (1) by heating or irradiation with light to obtain a liquid crystal / polymer composite material.

8. The preparation method according to claim 7, wherein: The liquid crystal molecules in step (1) include chiral compounds; and step (2) further includes: vertically aligning the liquid crystal molecules before heating or irradiation, or vertically aligning the liquid crystal molecules after curing the prepolymer solution and then heating or irradiating the liquid crystal molecules for a second time. 9 . A dimming film comprising the composite material according to claim 1 or the composite material obtained according to the preparation method according to claim 7 .

10. Use of the liquid crystal / polymer composite material according to claim 1 or the dimming film according to claim 9 in energy saving of automobiles and buildings.

Citation Information

Patent Citations

  • Process for preparing high polymer dispersed liquid crystal film material

    CN101007949A

  • Reverse type electric-control liquid-crystal light adjusting film and preparation method thereof

    CN106405916A

  • Liquid crystal light adjusting film with temperature control and electric control functions and preparation method thereof

    CN106526945A

  • Trans electronic control liquid crystal light dimming film and preparation method thereof

    CN106886102A

  • Electrically controlled dimming film and preparing method thereof

    CN108663828A