Light / moisture-curable resin composition, adhesive for electronic component, cured body, and electronic component

By adjusting the energy storage modulus and tanδ of the photomoisture-curing resin composition, the problem of insufficient initial adhesive strength of the photomoisture-curing adhesive is solved, high initial and final adhesive strength is achieved, and component adhesion is improved Workability and firmness of the connection.

CN118878751APending Publication Date: 2024-11-01SEKISUI CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411201340.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2020-05-15
Filing Date
2021-05-14
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The initial adhesive force of the light-moisture-curing adhesive is insufficient just after being bonded, resulting in poor workingability and it is difficult to quickly bond the components.

Method used

By adjusting the energy storage modulus (G') of the photomoisture curing resin composition at 25°C and tanδ at 75°C, it has high initial adhesion after photocuring, specific measures include the use of radical polymerization The energy storage modulus at 25°C is ensured to be 250 kPa or above and tan δ at 75°C is 1.0 or above, and dynamic viscoelasticity measurement is performed after ultraviolet irradiation.

Benefits of technology

The photomoisture-curing resin composition has excellent initial adhesive force just after photocuring, which improves workability and final adhesive force, and ensures firm bonding of the components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005017919120000181
    Figure BDA0005017919120000181
  • Figure BDA0005017919120000211
    Figure BDA0005017919120000211
  • Figure BDA0005017919120000361
    Figure BDA0005017919120000361
Patent Text Reader

Abstract

This light / moisture-curable resin composition contains a radical-polymerizable compound (A), a moisture-curable resin (B), and a photopolymerization initiator (C), and the light / moisture-curable resin composition is cured by irradiating the light / moisture-curable resin composition with ultraviolet light of 1000 mJ / cm2. The storage modulus (G ') at 25 DEG C when measured by a dynamic viscoelasticity measurement device at 1 Hz is 250 kPa or more, and the tan [delta] at 75 DEG C is 1.0 or more.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention of this application is a divisional application of the application with application number 202180016343.5, invention name “Light moisture curing resin composition, adhesive for electronic components, cured body and electronic components”, and application date May 14, 2021. Technical Field

[0002] The present invention relates to an optical moisture curing resin composition, an adhesive for electronic components, a cured product, and an electronic component. Background Art

[0003] In recent years, in electronic components such as semiconductor chips, high integration and miniaturization are required. For example, sometimes a plurality of thin semiconductor chips are bonded via an adhesive layer to form a stack of semiconductor chips. In addition, in the current era where various mobile devices with display elements have become popular, as a method of miniaturizing display elements, a narrow frame of the image display part (hereinafter also referred to as a "narrow frame design") is implemented. In these uses, along with miniaturization and narrow frame, attempts are being made to use optical moisture curing adhesives instead of double-sided tapes.

[0004] As an optical moisture curing adhesive, for example, Patent Document 1 discloses an optical moisture curing resin composition containing a radical polymerizable compound, a moisture curing polyurethane resin, and a photo radical polymerization initiator, wherein the moisture curing polyurethane resin contains a moisture curing polyurethane resin having a weight average molecular weight of 2000 or more. In addition, Patent Document 2 discloses a reactive hot melt adhesive composition containing a urethane prepolymer, a urethane (meth)acrylate having a (meth)acryloyl group, and a photopolymerization initiator.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2016-074781

[0008] Patent Document 2: Japanese Patent Application Publication No. 2019-006854 Summary of the invention

[0009] Problems to be solved by the invention

[0010] However, unlike double-sided tapes, optical moisture curing adhesives do not exhibit sufficient adhesive strength (initial adhesive strength) immediately after bonding, so it takes time to bond components together, which has problems in workability. For example, in Patent Documents 1 and 2, although it is shown that a certain adhesive strength is exhibited after light irradiation, the initial adhesive strength is sometimes insufficient.

[0011] Therefore, an object of the present invention is to provide a light moisture curable resin composition which exhibits high adhesive strength immediately after photocuring and can improve workability and the like.

[0012] Means for solving problems

[0013] As a result of intensive research, the inventors of the present application have found that the above-mentioned problems can be solved by setting the storage modulus (G') at 25°C and tan δ at 75°C of a photocured optical moisture curable resin composition within certain ranges, thereby completing the following invention. That is, the present invention provides the following [1] to

[25] .

[0014] [1] An optical moisture curable resin composition comprising a radical polymerizable compound (A), a moisture curable resin (B), and a photopolymerization initiator (C),

[0015] The optical moisture curable resin composition is irradiated with 1000 mJ / cm 2 In a state where the film is photocured by ultraviolet rays, the storage modulus (G') at 25°C when measured at 1 Hz by a dynamic viscoelasticity measuring device is 250 kPa or more, and the tan δ at 75°C is 1.0 or more.

[0016] [2] The optical moisture curable resin composition according to the above [1] is applied to an aluminum substrate with a line width of 1.0 mm and irradiated with 1000 mJ / cm 2 The glass plates were pressed at 0.08 MPa for 120 seconds under a state of photocuring by ultraviolet rays. At this time, if the average width of the bonding portion on the glass plate side is set to a and the average width of the bonding portion on the aluminum substrate side is set to b, a / b is 0.58 to 0.99.

[0017] [3] The optical moisture-curable resin composition according to [1] or [2] above, wherein the moisture-curable resin (B) comprises a moisture-curable polyurethane resin.

[0018] [4] The optical moisture-curable resin composition according to [3] above, wherein the moisture-curable polyurethane resin is a moisture-curable polyurethane resin having at least any one of a polycarbonate skeleton, a polyether skeleton, and a polyester skeleton.

[0019] [5] The optical moisture-curable resin composition according to [3] or [4] above, wherein the moisture-curable polyurethane resin is a moisture-curable polyurethane resin having a polycarbonate skeleton.

[0020] [6] The optical moisture curable resin composition according to any one of [1] to [5] above, wherein the weight average molecular weight of the moisture curable resin (B) is 7,500 to 24,000.

[0021] [7] The optical moisture curable resin composition according to any one of [1] to [6] above, wherein the radically polymerizable compound (A) contains a monofunctional radically polymerizable compound.

[0022] [8] The optical moisture curable resin composition according to [7] above, comprising 90 parts by mass or more of a monofunctional radical polymerizable compound based on 100 parts by mass of the radical polymerizable compound (A).

[0023] [9] The optical moisture curable resin composition according to [7] or [8] above, wherein the monofunctional radical polymerizable compound contains a nitrogen-containing compound.

[0024]

[10] The optical moisture curable resin composition according to the above [9], wherein the monofunctional radical polymerizable compound contains a chain nitrogen-containing compound.

[0025]

[11] The optical moisture curable resin composition according to [9] or

[10] above, wherein the monofunctional radical polymerizable compound includes a nitrogen-containing compound having a cyclic structure.

[0026]

[12] The optical moisture curable resin composition according to

[11] above, wherein the mass ratio (cyclic / chain) of the nitrogen-containing compound having a cyclic structure to the chain nitrogen-containing compound is 0.1 to 2.0.

[0027]

[13] The optical moisture curable resin composition according to any one of [9] to

[12] above, wherein the content of the nitrogen-containing compound as a monofunctional radical polymerizable compound is 10 to 95 parts by mass relative to 100 parts by mass of the radical polymerizable compound (A).

[0028]

[14] The optical moisture curable resin composition according to any one of [9] to

[13] above, wherein the monofunctional radical polymerizable compound further includes a monofunctional (meth)acrylate compound in addition to the nitrogen-containing compound.

[0029]

[15] The optical moisture curable resin composition according to

[14] above, wherein the monofunctional (meth)acrylate compound is at least one selected from the group consisting of alkyl (meth)acrylates, (meth)acrylates containing an alicyclic structure, and (meth)acrylates containing an aromatic ring.

[0030]

[16] The optical moisture curable resin composition according to the above

[15] , wherein the total content of the alkyl (meth)acrylate, the (meth)acrylate containing an alicyclic structure, and the (meth)acrylate containing an aromatic ring is 5 to 90 parts by mass based on 100 parts by mass of the radical polymerizable compound (A).

[0031]

[17] The optical moisture curable resin composition according to any one of [1] to

[16] above, wherein the mass ratio (B / A) of the moisture curable resin (B) to the radical polymerizable compound (A) is 30 / 70 to 90 / 10.

[0032]

[18] The optical moisture curable resin composition according to any one of [1] to

[17] above, further comprising a filler (D).

[0033]

[19] The optical moisture curable resin composition according to any one of [1] to

[18] above, wherein the photopolymerization initiator (C) is at least one selected from the group consisting of benzophenone compounds, acetophenone compounds, alkylphenone photopolymerization initiators, acylphosphine oxide compounds, titanocene compounds, oxime ester compounds, benzoin ether compounds, and thioxanthone.

[0034]

[20] The optical moisture curable resin composition according to any one of [1] to

[19] above, wherein the initial adhesive strength is 0.25 MPa or more.

[0035]

[21] The optical moisture curable resin composition according to any one of [1] to

[20] above, wherein the final adhesive strength is 2.0 MPa or more.

[0036]

[22] The optical moisture curable resin composition according to any one of [1] to

[21] above, wherein the viscosity measured using a cone and plate viscometer at 25° C. and 5.0 rpm is 35 Pa·s to 600 Pa·s.

[0037]

[23] An adhesive for electronic components, comprising the optical moisture curable resin composition according to any one of [1] to

[22] .

[0038]

[24] A cured product of the optical moisture curable resin composition according to any one of [1] to

[22] above.

[0039]

[25] An electronic component comprising the cured product according to

[24] above.

[0040] Effects of the Invention

[0041] According to the present invention, there is provided an optical moisture curable resin composition which exhibits excellent adhesive strength even immediately after photocuring and can improve workability and the like. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] [ Figure 1 ] is a conceptual diagram showing the method for measuring the internal-external ratio a / b.

[0043] [ Figure 2 ] is a schematic diagram showing the adhesion test method. Figure 2 (a) is a top view, Figure 2 (b) is a side view. DETAILED DESCRIPTION

[0044] Hereinafter, the present invention will be described in detail with reference to embodiments.

[0045] <Optical moisture curing resin composition>

[0046] The optical moisture curable resin composition of the present invention contains a radical polymerizable compound (A), a moisture curable resin (B), and a photopolymerization initiator (C).

[0047] The light moisture curable resin composition of the present invention is irradiated with 1000mJ / cm 2 In a state where the film is photocured by ultraviolet rays, the storage modulus (G') at 25°C when measured at 1 Hz using a dynamic viscoelasticity measuring device is 250 kPa or more, and the tan δ at 75°C is 1.0 or more.

[0048] The optical moisture curable resin composition of the present invention, when the storage modulus (G') at 25°C and tan δ at 75°C in the state of being photocured as described above are both above a certain value, will disintegrate to a certain extent when a moderate pressure acts just after photocuring, making it easy to adhere to the adherend, and will also show a certain cohesive force when shear stress acts. Therefore, the adhesive force (initial adhesive force) just after photocuring can be excellent.

[0049] [Storage modulus (G')]

[0050] The optical moisture curable resin composition of the present invention is a composition having a storage modulus (G') at 25°C measured in a state of being photocured as described above of 250 kPa or more. If the storage modulus (G') at 25°C is less than 250 kPa, the bulk strength after photocuring becomes low, which makes it difficult to increase the initial adhesive force.

[0051] From the viewpoint of improving bulk strength and thus initial adhesive force, the storage modulus (G') at 25°C is preferably 350 kPa or more, more preferably 500 kPa or more, further preferably 600 kPa or more, and further more preferably 700 kPa or more.

[0052] From the viewpoint of easily developing certain adhesiveness even immediately after photocuring, the storage modulus (G') at 25°C is preferably 4000 kPa or less, more preferably 3500 kPa or less, further preferably 3000 kPa or less, and further more preferably 2500 kPa or less.

[0053] [tanδ]

[0054] The optical moisture curing resin composition of the present invention is irradiated with 1000mJ / cm 2 In a state where the photocured resin composition is subjected to ultraviolet light, the tan δ at 75°C measured at 1 Hz using a dynamic viscoelasticity measuring device is 1.0 or more. If the tan δ at 75°C becomes less than 1.0, the photocured optical moisture curable resin composition is easy to rebound when compressed and is difficult to disintegrate, making it difficult to increase the initial adhesive force.

[0055] From the viewpoint of improving the initial adhesive force, tanδ at 75°C is preferably 1.05 or more, more preferably 1.1 or more, and even more preferably 1.2 or more. In addition, from the viewpoint of preventing excessive disintegration during compression and a decrease in the initial adhesive force, tanδ at 75°C is preferably 2.0 or less, more preferably 1.8 or less, and even more preferably 1.6 or less.

[0056] It should be noted that the storage modulus (G') at 25°C and tanδ at 75°C can be adjusted by the type, molecular weight, blending amount of the moisture-curable resin (B), the type and blending amount of the radical polymerizable compound (A). For example, if the molecular weight of the moisture-curable resin (B) is increased, the storage modulus (G') at 25°C tends to increase. In addition, if a large amount of a homopolymer having a large tanδ at 75°C is contained as a radical polymerizable compound (A), there is a tendency for the above-mentioned tanδ of the light moisture curable resin composition to increase. In addition, if a large amount of a monofunctional monomer is mixed as a radical polymerizable compound (A), there is a tendency for the above-mentioned tanδ to increase. In addition, if the molecular weight of the moisture-curable resin (B) is within a certain range, tanδ is easily within a specified range.

[0057] In addition, the storage modulus (G') and tan δ of the optical moisture curable resin composition can be measured as follows.

[0058] The optical moisture curable resin composition was applied to a viscoelasticity measurement jig and a 1000 mW UV-LED lamp was used to irradiate the resin composition at 1000 mJ / cm 2 The sample for evaluation was placed in a dynamic viscoelasticity measuring device within 30 seconds after the ultraviolet irradiation, and the storage modulus (G') and tan δ were measured at 10 to 100°C, heating rate = 5°C / min, frequency F = 1 Hz, and shear mode.

[0059] [Viscosity at 25°C]

[0060] The optical moisture curable resin composition of the present invention preferably has a viscosity measured using a cone and plate viscometer at 25° C. and 5.0 rpm (hereinafter also referred to as “25° C. viscosity”) of 35 Pa·s to 600 Pa·s.

[0061] The 25°C viscosity of the above-mentioned moisture-curable resin composition is a value measured under high shear of 5.0 rpm without light curing and moisture curing, and is a viscosity that is not easily affected by fillers. Therefore, if the 25°C viscosity is 35 Pa·s or more, there is a tendency for the low molecular weight components contained in the moisture-curable resin (B) etc. to decrease, and the moisture-curable resin (B) etc. is not easy to seep into the interface after light irradiation, and it is easy to increase the initial adhesion. That is, if the low molecular weight moisture-curable resin (B) etc. is not easy to seep into the interface after light irradiation, it is not easy to slide between it and the adherend, and it is easy to show adhesion, thereby easily improving the initial adhesion. In addition, even if the above-mentioned 25°C viscosity becomes less than 600 Pa·s, it is easy to show the adhesion originally possessed by the moisture-curable resin (B), etc., thereby becoming easy to increase the initial adhesion and the final adhesion described later.

[0062] Furthermore, by setting the viscosity at 25° C. to 35 Pa·s to 600 Pa·s, it is less likely that the liquid will drip or that coating cannot be performed at room temperature will occur, thereby improving workability.

[0063] The optical moisture curable resin composition has a 25°C viscosity of more preferably 40 Pa·s or more, further preferably 45 Pa·s or more, further preferably 90 Pa·s or more, further preferably 110 Pa·s or more, and more preferably 500 Pa·s or less, further preferably 350 Pa·s or less, further preferably 230 Pa·s or less. If the 25°C viscosity is within the above range, workability and initial adhesive strength are easily improved.

[0064] In addition, if it is set below the above upper limit, the molecular weight of the moisture-curable resin (A) can be prevented from being excessively increased, so that the initial adhesive force is easily increased, and further, the adhesive force is sufficiently increased by moisture curing, and the final adhesive force is also easily increased. It should be noted that the so-called final adhesive force refers to the adhesive force of the light moisture curable resin composition after light curing and moisture curing, and the details are described later.

[0065] [Inside-outside ratio a / b]

[0066] The optical moisture curable resin composition of the present invention is applied linearly to an aluminum substrate under the specified conditions described below, and when a glass plate is further pressed after being photocured using UV, when the average width of the bonding portion on the glass plate side is set to a and the average width of the bonding portion on the aluminum substrate side is set to b, a / b (also referred to as "inside-outside ratio a / b") is preferably 0.58 to 0.99.

[0067] The optical moisture curable resin composition of the present invention, when the above-mentioned internal and external ratio a / b is 0.58 or more, has a larger internal and external ratio a / b than conventional optical moisture curable resin compositions, and is easily disintegrated immediately after photocuring, and the adhesion of the interface with respect to the adherend becomes higher, and the initial adhesive force with respect to the adherend is easily increased. In addition, by making the internal and external ratio a / b 0.99 or less, it is possible to prevent the cohesive force of the optical moisture curable resin composition immediately after photocuring from becoming smaller, or from excessively disintegrating to reduce the initial adhesive force.

[0068] The above-mentioned inside-outside ratio a / b is more preferably 0.63 or more, and further preferably 0.66 or more, and more preferably 0.95 or less, and further preferably 0.93 or less. If the inside-outside ratio a / b is within these ranges, the initial bonding strength can be easily improved.

[0069] In the present invention, the internal and external ratio a / b is measured as follows. Figure 1 As shown in (a), a moisture curable resin composition 10 is applied to an aluminum substrate 11 with a line width of 1.0 mm. Here, the line width of 1.0 mm does not need to be exactly 1.0 mm, and an error of 1.0 ± 0.1 mm may exist. Figure 1 As shown in (b), the moisture curable resin composition 10 is irradiated with 1000 mJ / cm 2 The moisture-curable resin composition 10 is cured by ultraviolet light. Then, immediately (within 10 seconds), Figure 1As shown in (c), a glass plate 12 is superimposed on a moisture-curable resin composition 10, and the glass plate 12 is pressed at 0.08 MPa for 120 seconds relative to the coating area of ​​the moisture-curable resin composition 10. After pressing, the width a1 of the bonding portion of the moisture-curable resin composition 10 with the glass plate 12 is measured. The width a1 is measured at 5 points, and its average value is taken as the average width a. In addition, the width b1 of the bonding portion of the moisture-curable resin composition 10 with the aluminum substrate 11 is measured. The width b1 is measured at 5 points, and its average value is taken as the average width b, and the inside and outside ratio a / b is calculated from the average widths a and b. It should be noted that the pressing is performed using a weight, and the widths a1 and b1 can be measured 5 minutes after the weight is removed.

[0070] The internal and external ratio a / b can be adjusted to the above range by adjusting the type of free radical polymerizable compound, etc. For example, when the light moisture curable resin composition contains a large amount of monofunctional free radical polymerizable compounds as free radical polymerizable compounds, the proportion of the cross-linked structure formed after photocuring becomes less, so the internal and external ratio a / b can be increased. In addition, for example, even if the light moisture curable resin composition contains a large amount of free radical polymerizable compounds with a low glass transition temperature of the homopolymer as a free radical polymerizable compound, the cured product after photocuring becomes soft, so the internal and external ratio a / b can be increased. In addition, it can also be adjusted by the weight average molecular weight of the moisture curable resin (B).

[0071] [Adhesion]

[0072] The optical moisture curable resin composition of the present invention preferably has an initial adhesive force of 0.25 MPa or more. In addition, the optical moisture curable resin composition of the present invention preferably has a final adhesive force of 2.0 MPa or more.

[0073] It should be noted that the initial adhesive force refers to the adhesive force at 25°C just after the optical moisture curable resin composition is photocured, and the final adhesive force refers to the adhesive force after the optical moisture curable resin composition is photocured and then left under the conditions of 25°C and 50 RH% for 24 hours. Details of the method for measuring the initial adhesive force and the final adhesive force are described in the examples described below.

[0074] If the initial adhesive force of the light moisture curable resin composition at 25°C is 0.25 MPa or more, the adherends can be temporarily bonded to each other with a high adhesive force immediately after light curing, and the workability during temporary bonding is improved. In addition, if the final adhesive force is 2.0 MPa or more, the adherends can be firmly joined to each other by formal bonding by moisture curing after temporary bonding.

[0075] In order to further improve the bonding stability during temporary bonding, the initial bonding strength of the optical moisture curing resin composition is more preferably 0.4 MPa or more. In addition, the initial bonding strength is not particularly limited, and may be, for example, less than 1.5 MPa in order to facilitate re-bonding during temporary bonding.

[0076] In addition, in order to more firmly bond the adherends to each other after formal bonding, the final adhesive force of the optical moisture curing resin composition is more preferably 3.5 MPa or more. In addition, the higher the final adhesive force, the better, and there is no particular limitation, for example, 20 MPa or less, and it can also be 10 MPa or less.

[0077] Hereinafter, each component contained in the optical moisture curable resin composition is demonstrated in detail.

[0078] [Radical polymerizable compound (A)]

[0079] The optical moisture curable resin composition of the present invention contains a free radical polymerizable compound (A). The optical moisture curable resin composition is given photocurability by containing the free radical polymerizable compound (A). Since the optical moisture curable resin composition is photocurable, a certain adhesive force can be given only by light irradiation, and thus appropriate initial adhesive force can be ensured.

[0080] The radical polymerizable compound (A) may have a radical polymerizable functional group in the molecule. A compound having an unsaturated double bond as a radical polymerizable functional group is suitable, and examples thereof include a (meth)acryloyl group, a vinyl group, a styryl group, and an allyl group.

[0081] Among the above-mentioned groups, (meth)acryloyl is suitable from the viewpoint of adhesion, that is, the free radical polymerizable compound (A) preferably contains a compound having a (meth)acryloyl. It should be noted that, hereinafter, the compound having a (meth)acryloyl is also referred to as a "(meth)acrylic compound". In addition, in this specification, "(meth)acryloyl" refers to acryloyl or (meth)acryloyl, "(meth)acrylic-" refers to "acrylic-" or "methacrylic-", and other similar terms are the same.

[0082] The radical polymerizable compound (A) may include one or both of a monofunctional radical polymerizable compound having one radical polymerizable functional group in one molecule and a polyfunctional radical polymerizable compound having two or more radical polymerizable functional groups in one molecule. However, from the viewpoint of improving the tanδ after the above-mentioned photocuring and improving the initial adhesion of the light moisture curing resin composition, it is preferred to include a monofunctional radical polymerizable compound. In addition, among the radical polymerizable compounds (A), as a monofunctional radical polymerizable compound, it is more preferred to include at least a monofunctional (meth) acrylic compound as a (meth) acrylic compound. It should be noted that the monofunctional radical polymerizable compound may also be a prepolymer having a repeating unit after polymerization, but it is generally appropriate to use a monofunctional monomer having no repeating unit.

[0083] In order to improve the tanδ of the optical moisture curable resin composition after photocuring and improve the initial adhesive force, the optical moisture curable resin composition preferably contains a large amount of monofunctional free radical polymerizable compounds. Specifically, the optical moisture curable resin composition preferably contains 90 parts by mass or more of the monofunctional free radical polymerizable compound, preferably contains 95 parts by mass or more of the monofunctional free radical polymerizable compound, and further preferably contains 100 parts by mass of the monofunctional free radical polymerizable compound, relative to 100 parts by mass of the free radical polymerizable compound (A).

[0084] [Monofunctional radical polymerizable compound]

[0085] (Nitrogen-containing compounds)

[0086] The radical polymerizable compound (A) preferably contains a nitrogen-containing compound as a monofunctional radical polymerizable compound. By using a nitrogen-containing compound, the initial adhesion of the light moisture curable resin composition becomes good. After being applied to the adherend, the light moisture curable resin composition is irradiated with active energy rays such as ultraviolet rays to perform photocuring. At this time, it is usually more common to perform photocuring in the presence of oxygen as described later. If the radical polymerizable compound (A) contains a nitrogen-containing compound, photocuring is appropriately performed even in the presence of oxygen, thereby inferring that the initial adhesion becomes good.

[0087] The nitrogen-containing compound may contain one or both of a chain nitrogen-containing compound and a nitrogen-containing compound having a cyclic structure, but from the viewpoint of improving the initial adhesion of the optical moisture curable resin composition, it is preferred to contain a nitrogen-containing compound having a cyclic structure, and it is more preferred to use a chain nitrogen-containing compound and a nitrogen-containing compound having a cyclic structure in combination.

[0088] As the nitrogen-containing compound with a cyclic structure, there can be enumerated the nitrogen-containing compounds with lactam structure such as N-vinyl pyrrolidone, N-vinyl-ε-caprolactam, compounds containing morpholine skeletons such as N-acryloyl morpholine, cyclic imide compounds such as N-(methyl)acryloyloxyethyl hexahydrophthalimide, etc. Among these compounds, compounds containing amide groups such as N-vinyl caprolactam are further preferred. It should be noted that in this specification, the nitrogen-containing compound with a cyclic structure is also referred to as a cyclic nitrogen-containing compound, and the free radical polymerizable compound in which the nitrogen atom is contained in the atoms constituting the ring itself is regarded as a cyclic nitrogen-containing compound, and other nitrogen-containing compounds are regarded as chain nitrogen-containing compounds.

[0089] Examples of the chain nitrogen-containing compound include chain (meth)acrylates containing an amino group such as dimethylamino (meth)acrylate, diethylamino (meth)acrylate, aminomethyl (meth)acrylate, aminoethyl (meth)acrylate, and dimethylaminoethyl (meth)acrylate; chain (meth)acrylamide compounds such as diacetone acrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, N-isopropylacrylamide, N-hydroxyethylacrylamide, acrylamide, and methacrylamide; and N-vinylacetamide.

[0090] In addition, as a chain nitrogen-containing compound, a monofunctional carbamate (meth) acrylate may also be used. By using a monofunctional carbamate (meth) acrylate, when a polyurethane resin, particularly a polyurethane resin having a polycarbonate skeleton, is used as the moisture-curable resin (B), the compatibility with the moisture-curable resin (B) becomes good, and the initial adhesive force is easily improved. In addition, the polarity of carbamate (meth) acrylate is relatively high, so it is easy to increase the adhesive force relative to glass.

[0091] As the monofunctional urethane (meth)acrylate, for example, one obtained by reacting a (meth)acrylic acid derivative having a hydroxyl group with an isocyanate compound can be used.

[0092] Examples of the (meth)acrylic acid derivative having a hydroxyl group include mono(meth)acrylates of diols such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol and polyethylene glycol; and mono(meth)acrylates of triols such as trimethylolethane, trimethylolpropane and glycerol.

[0093] Examples of the isocyanate compound for obtaining the urethane (meth)acrylate include aliphatic monoisocyanates such as butane isocyanate, hexane isocyanate, and decane isocyanate, and cyclopentane isocyanate, cyclohexane isocyanate, and cyclic aliphatic monoisocyanates such as isophorone monoisocyanate.

[0094] More specifically, the monofunctional urethane (meth)acrylate is preferably a urethane (meth)acrylate obtained by reacting the above-mentioned monoisocyanate compound with a mono(meth)acrylate of a diol, and a suitable specific example thereof includes 1,2-ethanediol 1-acrylate 2-(N-butyl carbamate).

[0095] Among the above compounds, the chain nitrogen-containing compound preferably includes a monofunctional urethane (meth)acrylate, and it is also preferred to use a monofunctional urethane (meth)acrylate in combination with a compound other than a monofunctional urethane (meth)acrylate such as a (meth)acrylamide compound.

[0096] From the viewpoint of improving the initial adhesion of the optical moisture curable resin composition, the content of the nitrogen-containing compound as a monofunctional free radical polymerizable compound in the optical moisture curable resin composition is preferably 10 parts by mass or more, more preferably 30 parts by mass or more, further preferably 50 parts by mass or more, and most preferably 60 parts by mass or more, relative to 100 parts by mass of the free radical polymerizable compound (A). In addition, in order to contain an appropriate amount of free radical polymerizable compounds (A) other than the nitrogen-containing compound, the content of the nitrogen-containing compound as the monofunctional free radical polymerizable compound is preferably 95 parts by mass or less, more preferably 90 parts by mass or less, and further preferably 85 parts by mass or less.

[0097] When the monofunctional radical polymerizable compound contains a chain nitrogen-containing compound and a nitrogen-containing compound having a cyclic structure, the mass ratio of the nitrogen-containing compound having a cyclic structure to the chain nitrogen-containing compound in the monofunctional radical polymerizable compound (cyclic / chain) is preferably 0.1 to 2.0, more preferably 0.2 to 1.5, and further preferably 0.4 to 1.2. By making the mass ratio of the cyclic / chain structure within the above range, the initial adhesion of the optical moisture curing type resin composition can be improved.

[0098] (Monofunctional radical polymerizable compounds other than nitrogen-containing compounds)

[0099] The monofunctional radical polymerizable compound contained in the radical polymerizable compound (A) preferably includes a compound other than the above-mentioned nitrogen-containing compound (hereinafter also referred to as a nitrogen-free compound). By making the radical polymerizable compound (A) contain a nitrogen-free compound as a monofunctional radical polymerizable compound, it is easy to improve adhesion, etc.

[0100] The nitrogen-free compound is not particularly limited as long as it is a compound having a radical polymerizable functional group, but is preferably a monofunctional (meth)acrylic compound, and among these, a (meth)acrylate compound is more preferably used.

[0101] Examples of the monofunctional (meth)acrylate compound include alkyl (meth)acrylates, (meth)acrylates containing an alicyclic structure, (meth)acrylates containing an aromatic ring, etc. These may be used alone or in combination of two or more, but among these, it is preferred to use one or both of the alkyl (meth)acrylates and the (meth)acrylates containing an aromatic ring.

[0102] The total content of the (meth) acrylate alkyl ester, the (meth) acrylate containing an alicyclic structure, and the (meth) acrylate containing an aromatic ring in the radical polymerizable compound (A) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and further preferably 15 parts by mass or more, relative to 100 parts by mass of the radical polymerizable compound (A). In addition, the above content is preferably 90 parts by mass or less, more preferably 70 parts by mass or less, further preferably 60 parts by mass or less, and most preferably 40 parts by mass or less.

[0103] Examples of the alkyl (meth)acrylate include alkyl (meth)acrylates having an alkyl group with 1 to 18 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, isomyristyl (meth)acrylate, and stearyl (meth)acrylate.

[0104] Examples of the (meth)acrylate containing an alicyclic structure include cyclohexyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, and dicyclopentenyl (meth)acrylate.

[0105] Examples of the (meth)acrylate containing an aromatic ring include benzyl (meth)acrylate, phenylalkyl (meth)acrylate such as 2-phenylethyl (meth)acrylate, and phenoxyalkyl (meth)acrylate such as phenoxyethyl (meth)acrylate.

[0106] As the monofunctional (meth)acrylate compound, compounds other than alkyl (meth)acrylates, (meth)acrylates containing an alicyclic structure, and (meth)acrylates containing an aromatic ring may be used. For example, (meth)acrylates containing a cyclic ether group may be used.

[0107] Examples of the cyclic ether group-containing (meth)acrylate include (meth)acrylates having an epoxy ring, an oxetane ring, a tetrahydrofuran ring, a dioxolane ring, a dioxane ring, and the like.

[0108] As (meth)acrylates containing epoxy rings, for example, glycidyl (meth)acrylate can be mentioned. As (meth)acrylates containing oxetane rings, (meth)acrylate (3-ethyloxetane-3-yl)methyl can be mentioned. As (meth)acrylates containing tetrahydrofuran rings, (meth)acrylate tetrahydrofurfuryl ester, (meth)acrylate polymers of tetrahydrofurfuryl alcohol, etc. can be mentioned. As (meth)acrylates containing dioxolane rings, (meth)acrylate (2-methyl-2-ethyl-1,3-dioxolane-4-yl)methyl ester, (meth)acrylate (2,2-cyclohexyl-1,3-dioxolane-4-yl)methyl ester, etc. can be mentioned. As (meth)acrylates having dioxane rings, cyclic trimethylolpropane formal (meth)acrylate can be mentioned.

[0109] As the (meth)acrylate containing a cyclic ether group, it is preferable to use either an oxetane ring-containing (meth)acrylate or a tetrahydrofuran ring-containing (meth)acrylate, but it is also preferable to use them in combination.

[0110] In addition, as the monofunctional (meth)acrylate compound, hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate, alkoxyalkyl (meth)acrylates such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, and 2-butoxyethyl (meth)acrylate, alkoxyethylene glycol (meth)acrylates such as methoxyethylene glycol (meth)acrylate and ethoxyethylene glycol (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, ethylcarbitol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, ethoxytriethylene glycol (meth)acrylate, ethoxypolyethylene glycol (meth)acrylate, polyoxyethylene (meth)acrylates such as ethoxypolyethylene glycol (meth)acrylate, and the like can also be used.

[0111] As the monofunctional (meth)acrylic acid compound, a (meth)acrylic acid compound containing a carboxyl group such as acrylic acid or methacrylic acid can be used.

[0112] [Compounds other than monofunctional radical polymerizable compounds]

[0113] The radical polymerizable compound (A) may also contain a polyfunctional radical polymerizable compound as long as the effect of the present invention can be achieved. Examples of the polyfunctional radical polymerizable compound include bifunctional (meth)acrylate compounds, trifunctional or higher (meth)acrylate compounds, bifunctional or higher urethane (meth)acrylates, and the like.

[0114] Examples of the bifunctional (meth)acrylate compound include 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 2-n-butyl-2-ethyl-1,3-propanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, and tripropylene glycol di(meth)acrylate. di(meth)acrylate, polypropylene glycol di(meth)acrylate, ethylene oxide added bisphenol A di(meth)acrylate, propylene oxide added bisphenol A di(meth)acrylate, ethylene oxide added bisphenol F di(meth)acrylate, dihydroxymethyl dicyclopentadienyl di(meth)acrylate, neopentyl glycol di(meth)acrylate, (meth)acrylate 2-hydroxy-3-(meth)acryloyloxypropyl, carbonate diol di(meth)acrylate, polyether diol di(meth)acrylate, polyester diol di(meth)acrylate, polycaprolactone diol di(meth)acrylate, polybutadiene diol di(meth)acrylate, and the like.

[0115] Examples of the trifunctional or higher-functional (meth)acrylate compound include trimethylolpropane tri(meth)acrylate, ethylene oxide-added trimethylolpropane tri(meth)acrylate, propylene oxide-added trimethylolpropane tri(meth)acrylate, caprolactone-modified trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, glycerol tri(meth)acrylate, propylene oxide-added glycerol tri(meth)acrylate, tri(meth)acryloyloxyethyl phosphate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.

[0116] As the bifunctional or higher-functional urethane (meth)acrylate, for example, a urethane (meth)acrylate obtained by reacting a (meth)acrylic acid derivative having a hydroxyl group with an isocyanate compound can be used.

[0117] Examples of the (meth)acrylic acid derivative having a hydroxyl group include mono(meth)acrylates of diols such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, and polyethylene glycol; mono(meth)acrylates or di(meth)acrylates of triols such as trimethylolethane, trimethylolpropane, and glycerol; and epoxy(meth)acrylates such as bisphenol A epoxy(meth)acrylate.

[0118] Examples of the isocyanate compound for obtaining the urethane (meth)acrylate include polyisocyanate compounds such as isophorone diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, diphenylmethane-4,4′-diisocyanate (MDI), hydrogenated MDI, polymeric MDI, 1,5-naphthalene diisocyanate, norbornane diisocyanate, tolidine diisocyanate, xylylene diisocyanate (XDI), hydrogenated XDI, lysine diisocyanate, triphenylmethane triisocyanate, tris(isocyanatophenyl)phosphorothioate, tetramethylxylylene diisocyanate, and 1,6,11-undecane triisocyanate.

[0119] In addition, as the isocyanate compound, a chain-extended polyisocyanate compound obtained by reacting a polyol with an excess of an isocyanate compound may also be used. Here, as the polyol, for example, ethylene glycol, propylene glycol, glycerin, sorbitol, trimethylolpropane, carbonate diol, polyether diol, polyester diol, polycaprolactone diol, etc. may be mentioned.

[0120] By using these polyisocyanate compounds, polyfunctional urethane (meth)acrylate can be obtained.

[0121] [Moisture curable resin (B)]

[0122] As the moisture-curable resin (B) used in the present invention, for example, moisture-curable polyurethane resin, resin containing a hydrolyzable silyl group, moisture-curable cyanoacrylate resin, etc. can be mentioned, among which any one of moisture-curable polyurethane resin and resin containing a hydrolyzable silyl group is preferred, and moisture-curable polyurethane resin is more preferred. These can be used alone or in combination of two or more.

[0123] (Moisture curable polyurethane resin)

[0124] Moisture curable polyurethane resin can be obtained by reacting a polyol compound having more than two hydroxyl groups in one molecule with a polyisocyanate compound having more than two isocyanate groups in one molecule. Moisture curable polyurethane resin can have an isocyanate group in the molecule, and the isocyanate group in the molecule reacts with moisture in the air or in the adherend to be cured. Moisture curable polyurethane resin can have only one isocyanate group in one molecule, or it can have more than two isocyanate groups, but moisture curable polyurethane resin preferably has one or two isocyanate groups in one molecule. In addition, the isocyanate group is not particularly limited and can be provided at the end of the moisture curable polyurethane resin.

[0125] The reaction of the polyol compound and the polyisocyanate compound is usually performed within a range of [NCO] / [OH]=2.0 to 2.5 in terms of the molar ratio of the hydroxyl group (OH) in the polyol compound to the isocyanate group (NCO) in the polyisocyanate compound.

[0126] As the polyol compound that becomes the raw material of moisture-curable polyurethane resin, known polyol compounds commonly used in the manufacture of polyurethane can be used, for example, polyester polyol, polyether polyol, polyalkylene polyol, polycarbonate polyol, etc. These polyol compounds can be used alone or in combination of two or more.

[0127] The moisture-curable polyurethane resin is preferably at least one of a moisture-curable polyurethane resin having a polycarbonate skeleton, a polyether skeleton, or a polyester skeleton, more preferably at least one of a moisture-curable polyurethane resin having a polycarbonate skeleton or a polyether skeleton, and further preferably a moisture-curable polyurethane resin having a polycarbonate skeleton. The moisture-curable polyurethane resin has both excellent initial adhesion and final adhesion due to having a polycarbonate skeleton. It is also possible to provide an optical moisture-curable resin composition having excellent weather resistance, heat resistance, moisture resistance, etc. of a cured product.

[0128] (Moisture-curable polyurethane resin having a polycarbonate skeleton)

[0129] The moisture-curable polyurethane resin having a polycarbonate skeleton is a resin in which a polycarbonate skeleton is introduced into a polyurethane resin by using a polycarbonate polyol as the above-mentioned polyol compound. The moisture-curable polyurethane resin having a polycarbonate skeleton can be obtained by, for example, reacting a polycarbonate polyol having two or more hydroxyl groups in one molecule with a polyisocyanate compound having two or more isocyanate groups in one molecule.

[0130] The polycarbonate polyol is preferably a polycarbonate diol, and specific preferred examples of the polycarbonate diol include compounds represented by the following formula (1).

[0131]

[0132] In the formula (1), R is a divalent hydrocarbon group having 4 to 16 carbon atoms, and n is an integer of 2 to 500.

[0133] In formula (1), R is preferably an aliphatic saturated hydrocarbon group. By making R an aliphatic saturated hydrocarbon group, heat resistance is easily improved. In addition, it is not easy to produce yellowing due to thermal degradation, and weather resistance is also improved. R formed by an aliphatic saturated hydrocarbon group can have a chain structure or a cyclic structure, but from the viewpoint of easily making stress relaxation and flexibility good, it is preferably a chain structure. In addition, the chain structure R can be any shape of a straight chain or a branched chain.

[0134] n is preferably 5-200, more preferably 10-150, further preferably 20-50.

[0135] In addition, R contained in the polycarbonate polyol constituting the moisture curable polyurethane resin may be used alone or in combination of two or more. When two or more are used in combination, preferably at least a portion is a chain aliphatic saturated hydrocarbon group having 6 or more carbon atoms, and more preferably at least a portion is a chain aliphatic saturated hydrocarbon group having 7 or more carbon atoms.

[0136] By including a chain aliphatic saturated hydrocarbon group having 7 or more carbon atoms, stress relaxation and flexibility can be easily improved. When the polycarbonate diol is a compound represented by the above formula (1), the proportion of the chain aliphatic saturated hydrocarbon group having 7 or more carbon atoms is preferably 20 mol% to 100 mol%, more preferably 30 mol% to 100 mol%, and further preferably 50 mol% to 100 mol% relative to the R contained in the whole polycarbonate diol.

[0137] The chain aliphatic saturated hydrocarbon group having 7 or more carbon atoms preferably has 8 to 12 carbon atoms, and more preferably has 8 to 10 carbon atoms.

[0138] As a specific example of R, it can be a straight chain such as 1,4-butylene, pentylene, 1,6-hexylene, 1,7-heptylene, 1,8-octylene, 1,9-nonylene, 1,10-decylene, or a branched chain such as methylpentylene such as 3-methylpentylene, methyl-1,8-octylene. Multiple Rs in one molecule may be the same or different. Therefore, two or more Rs may be contained in one molecule, in which case, it is preferred that two or three Rs are contained in one molecule. For example, a polycarbonate polyol may be a copolymer containing Rs with a carbon number of 6 or less and Rs with a carbon number of 7 or more in one molecule, in which case any R may be a chain-like aliphatic saturated hydrocarbon group.

[0139] In addition, R may contain a linear aliphatic saturated hydrocarbon group or a branched aliphatic saturated hydrocarbon group. R in the polycarbonate polyol may contain a combination of a branched and a linear R, or a linear R alone.

[0140] In addition, the polycarbonate polyol may be used individually by 1 type, or may use 2 or more types together.

[0141] As the polyisocyanate compound serving as a raw material of the moisture-curable polyurethane resin, an aromatic polyisocyanate compound or an aliphatic polyisocyanate compound is preferably used.

[0142] Examples of the aromatic polyisocyanate compound include diphenylmethane diisocyanate, liquid modified products of diphenylmethane diisocyanate, polymeric MDI, toluene diisocyanate, and naphthalene-1,5-diisocyanate.

[0143] Examples of the aliphatic polyisocyanate compound include hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, lysine diisocyanate, norbornane diisocyanate, trans-cyclohexane-1,4-diisocyanate, isophorone diisocyanate, hydrogenated xylylene diisocyanate, hydrogenated diphenylmethane diisocyanate, cyclohexane diisocyanate, bis(isocyanatomethyl)cyclohexane, and dicyclohexylmethane diisocyanate.

[0144] As the polyisocyanate compound, aromatic polyisocyanate compounds are preferred from the viewpoint of being able to improve the adhesive force after full curing, and diphenylmethane diisocyanate and its modified products are more preferred. In addition, aliphatic polyisocyanate compounds are preferred from the viewpoint of easily imparting stress relaxation and flexibility to the cured product of the light moisture curable resin composition.

[0145] The polyisocyanate compound may be used alone or in combination of two or more.

[0146] (Moisture-curable polyurethane resin having a polyester skeleton)

[0147] The moisture-curable polyurethane resin having a polyester skeleton is a resin in which a polyester skeleton is introduced into a polyurethane resin by using a polyester polyol as the above-mentioned polyol compound. The moisture-curable polyurethane resin having a polyester skeleton can be obtained by reacting a polyester polyol having two or more hydroxyl groups in one molecule with a polyisocyanate compound having two or more isocyanate groups in one molecule.

[0148] Examples of the polyester polyol include polyester polyols obtained by reaction between a polycarboxylic acid and a polyol, and poly-ε-caprolactone polyols obtained by ring-opening polymerization of ε-caprolactone.

[0149] Examples of the polycarboxylic acid used as the raw material of the polyester polyol include phthalic acid, terephthalic acid, isophthalic acid, 1,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, decamethylene dicarboxylic acid, and dodecamethylene dicarboxylic acid. Among these polycarboxylic acids, phthalic acid or adipic acid is preferred from the viewpoint of being easy to further improve the adhesive force at high temperature.

[0150] Examples of the polyols used as the raw material of the polyester polyol include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, cyclohexanediol, etc. Among these polyols, 1,6-hexanediol or 1,4-butanediol is preferred from the viewpoint of further improving the adhesive force at high temperature.

[0151] In addition, the polyester polyol may be used individually by 1 type, or may use 2 or more types together.

[0152] (Moisture-curable polyurethane resin having a polyether skeleton)

[0153] The moisture-curable polyurethane resin having a polyether skeleton is a resin in which a polyether skeleton is introduced into a polyurethane resin by using a polyether polyol as the above-mentioned polyol compound. The polyurethane resin having a polyether skeleton can be obtained by reacting a polyether polyol having two or more hydroxyl groups in one molecule with a polyisocyanate compound having two or more isocyanate groups in one molecule.

[0154] Examples of the polyether polyol include polyethylene glycol, polypropylene glycol, ring-opening polymers of tetrahydrofuran, ring-opening polymers of 3-methyltetrahydrofuran, random copolymers or block copolymers thereof or derivatives thereof, and bisphenol-type polyoxyalkylene modified products. Among these polyether polyols, polypropylene glycol, ring-opening polymers of tetrahydrofuran, or ring-opening polymers of 3-methyltetrahydrofuran are preferred from the viewpoint of easily improving the coating properties of the optical moisture curable resin composition.

[0155] Here, the bisphenol type polyoxyalkylene modified body is a polyether polyol obtained by adding an alkylene oxide (e.g., ethylene oxide, propylene oxide, butylene oxide, isobutylene oxide, etc.) to the active hydrogen part of the bisphenol type molecular skeleton. The polyether polyol can be a random copolymer or a block copolymer. The above-mentioned bisphenol type polyoxyalkylene modified body preferably has one or more alkylene oxides added to both ends of the bisphenol type molecular skeleton.

[0156] The bisphenol type is not particularly limited, and examples thereof include A type, F type, and S type, and bisphenol A type is preferred.

[0157] Moreover, as a polyisocyanate compound, the above-mentioned polyisocyanate compounds can be used.

[0158] The moisture-curable polyurethane resin having a polyether skeleton preferably further comprises a resin obtained by using a polyol compound having a structure represented by the following formula (2). By using a polyol compound having a structure represented by the following formula (2), an optical moisture-curable resin composition having excellent adhesion and a cured product having softness and good stretchability can be obtained, which has excellent compatibility with the free radical polymerizable compound (A).

[0159] Among them, the resin using a polyether polyol formed from a ring-opening polymer compound of polypropylene glycol, tetrahydrofuran (THF) compound, or a ring-opening polymer compound of a tetrahydrofuran compound having a substituent such as a methyl group is preferred, and the ring-opening polymer compound of polypropylene glycol and tetrahydrofuran (THF) compound is more preferred. The ring-opening polymer compound of tetrahydrofuran (THF) compound is generally polytetramethylene ether glycol.

[0160] In addition, the polyether polyol may be used individually by 1 type, or may use 2 or more types together.

[0161]

[0162] In formula (2), R represents a hydrogen atom, a methyl group, or an ethyl group, l is an integer of 0 to 5, m is an integer of 1 to 500, and n is an integer of 1 to 10. l is preferably 0 to 4, m is preferably 50 to 200, and n is preferably 1 to 5. It should be noted that the case where l is 0 means that the carbon bonded to R is directly bonded to oxygen.

[0163] In the above, the total of n and l is more preferably 1 or more, and further preferably 1 to 3. In addition, R is more preferably a hydrogen atom or a methyl group, and particularly preferably a methyl group.

[0164] The above-mentioned moisture-curable polyurethane resin with polycarbonate, polyester or polyether skeleton can have two or more skeletons in the molecule, for example, can have polycarbonate skeleton and polyester skeleton. In this case, polycarbonate polyol and polyester polyol can be used as the above-mentioned polyol compound becoming raw material. Similarly, moisture-curable polyurethane resin with polyester skeleton and polyether skeleton etc. can also be used.

[0165] As described above, the moisture-curable polyurethane resin may be an isocyanate group-containing resin, but is not limited to the isocyanate group-containing resin and may be a hydrolyzable silyl group-containing polyurethane resin as described in the hydrolyzable silyl group-containing resin described later.

[0166] (Hydrolyzable silyl group-containing resin)

[0167] The hydrolyzable silyl group-containing resin used in the present invention is cured by the reaction of the hydrolyzable silyl group in the molecule with moisture in the air or in an adherend.

[0168] The hydrolyzable silyl group-containing resin may have only one hydrolyzable silyl group in one molecule, or may have two or more hydrolyzable silyl groups. Among them, it is preferred that the resin has hydrolyzable silyl groups at both ends of the main chain of the molecule.

[0169] It should be noted that the hydrolyzable silyl group-containing resin does not include a resin having an isocyanate group.

[0170] The hydrolyzable silyl group is represented by the following formula (3).

[0171] -SiR 1 3-a X a (3)

[0172] In formula (3), R 1 Each independently represents an optionally substituted alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, or -OSiR 2 3 (R 2 Each of the X's is independently a hydrocarbon group having 1 to 20 carbon atoms) and is a triorganosiloxy group. In the formula (3), each of the X's is independently a hydroxyl group or a hydrolyzable group. In the formula (3), a is an integer of 1 to 3.

[0173] The above-mentioned hydrolyzable group is not particularly limited, and for example, halogen atoms, alkoxy groups, alkenyloxy groups, aryloxy groups, acyloxy groups, ketoxime ester groups, amino groups, amide groups, acid amide groups, aminooxy groups, sulfhydryl groups, etc. can be cited. Wherein, from the aspect of high activity, halogen atoms, alkoxy groups, alkenyloxy groups, acyloxy groups are preferably used. In addition, from the aspect of gentle hydrolysis and easy operation, alkoxy groups such as methoxy groups and ethoxy groups are more preferably used, and methoxy groups and ethoxy groups are further preferably used. In addition, from the viewpoint of safety, it is preferred that the compound separated by reaction is ethanol, acetone, ethoxy, isopropyleneoxy groups, respectively.

[0174] The hydroxyl group or the hydrolyzable group may be bonded to one silicon atom in a range of 1 to 3. When two or more hydroxyl groups or the hydrolyzable groups are bonded to one silicon atom, these groups may be the same or different.

[0175] From the viewpoint of curability, a in the formula (3) is preferably 2 or 3, and particularly preferably 3. From the viewpoint of storage stability, a is preferably 2.

[0176] In addition, as R in the above formula (3), 1 Examples thereof include methyl, alkyl groups such as ethyl, cycloalkyl groups such as cyclohexyl, aryl groups such as phenyl, aralkyl groups such as benzyl, trimethylsilyloxy, chloromethyl, and methoxymethyl. Among them, methyl is preferred.

[0177] Examples of the hydrolyzable silyl group include methyldimethoxysilyl, trimethoxysilyl, triethoxysilyl, tri(2-propenyloxy)silyl, triacetoxysilyl, (chloromethyl)dimethoxysilyl, (chloromethyl)diethoxysilyl, (dichloromethyl)dimethoxysilyl, (1-chloroethyl)dimethoxysilyl, (1-chloropropyl)dimethoxysilyl, (methoxymethyl)dimethoxysilyl, and (methoxymethyl)diethoxysilyl. dimethoxysilyl, (ethoxymethyl)dimethoxysilyl, (1-methoxyethyl)dimethoxysilyl, (aminomethyl)dimethoxysilyl, (N,N-dimethylaminomethyl)dimethoxysilyl, (N,N-diethylaminomethyl)dimethoxysilyl, (N,N-diethylaminomethyl)diethoxysilyl, (N-(2-aminoethyl)aminomethyl)dimethoxysilyl, (acetoxymethyl)dimethoxysilyl, (acetoxymethyl)diethoxysilyl and the like.

[0178] Examples of the hydrolyzable silyl group-containing resin include a hydrolyzable silyl group-containing (meth)acrylic resin, an organic polymer having a hydrolyzable silyl group at a molecular chain terminal or at a molecular chain terminal portion, and a hydrolyzable silyl group-containing polyurethane resin.

[0179] The hydrolyzable silyl group-containing (meth)acrylic resin preferably has a repeating structural unit derived from a hydrolyzable silyl group-containing (meth)acrylic acid ester and / or an alkyl (meth)acrylate in the main chain.

[0180] Examples of the (meth)acrylate containing a hydrolyzable silyl group include 3-(trimethoxysilyl)propyl (meth)acrylate, 3-(triethoxysilyl)propyl (meth)acrylate, 3-(methyldimethoxysilyl)propyl (meth)acrylate, 2-(trimethoxysilyl)ethyl (meth)acrylate, 2-(triethoxysilyl)ethyl (meth)acrylate, 2-(methyldimethoxysilyl)ethyl (meth)acrylate, trimethoxysilylmethyl (meth)acrylate, triethoxysilylmethyl (meth)acrylate, and (methyldimethoxysilyl)methyl (meth)acrylate.

[0181] Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, and stearyl (meth)acrylate.

[0182] Specific examples of the method for producing a hydrolyzable silyl group-containing (meth)acrylic resin include a method for synthesizing a hydrolyzable silicon group-containing (meth)acrylate polymer described in International Publication No. 2016 / 035718.

[0183] The organic polymer having a hydrolyzable silyl group at a molecular chain terminal or at a molecular chain terminal site has a hydrolyzable silyl group at at least one of a main chain terminal and a side chain terminal.

[0184] The skeleton structure of the main chain is not particularly limited, and examples thereof include saturated hydrocarbon polymers, polyoxyalkylene polymers, (meth)acrylate polymers, and the like.

[0185] Examples of the polyoxyalkylene polymer include polymers having a polyoxyethylene structure, a polyoxypropylene structure, a polyoxybutylene structure, a polyoxytetramethylene structure, a polyoxyethylene-polyoxypropylene copolymer structure, and a polyoxypropylene-polyoxybutylene copolymer structure.

[0186] As a method for producing the above-mentioned organic polymer having a hydrolyzable silyl group at the molecular chain end or at the molecular chain end portion, specifically, for example, the method for synthesizing an organic polymer having only a crosslinkable silyl group at the molecular chain end or at the molecular chain end portion described in International Publication No. 2016 / 035718 can be cited. In addition, as another method for producing the above-mentioned organic polymer having a hydrolyzable silyl group at the molecular chain end or at the molecular chain end portion, for example, the method for synthesizing a polyoxyalkylene polymer containing a reactive silicon group described in International Publication No. 2012 / 117902 can be cited.

[0187] As a method for producing the above-mentioned polyurethane resin containing a hydrolyzable silyl group, for example, when a polyol compound and a polyisocyanate compound are reacted to produce a polyurethane resin, a method of further reacting a compound containing a silyl group such as a silane coupling agent, etc. Specifically, for example, a method for synthesizing a urethane oligomer having a hydrolyzable silyl group described in Japanese Patent Application Laid-Open No. 2017-48345, etc. can be mentioned.

[0188] Examples of the silane coupling agent include vinyl trichlorosilane, vinyl triethoxysilane, vinyl tri(β-methoxy-ethoxy)silane, β-(3,4-epoxycyclohexyl)-ethyl trimethoxysilane, γ-glycidoxypropyl trimethoxysilane, γ-glycidoxypropyl methyl diethoxysilane, γ-methacryloxypropyl trimethoxysilane, N-(β-aminoethyl)-γ-aminopropyl trimethoxysilane, N-(β-aminoethyl)-γ-aminopropyl trimethyl dimethoxysilane, N-phenyl-γ-aminopropyl trimethoxysilane, γ-chloropropyl trimethoxysilane, γ-mercaptopropyl trimethoxysilane, γ-aminopropyl trimethoxysilane, 3-isocyanate propyl trimethoxysilane, and 3-isocyanate propyl triethoxysilane. Among them, γ-mercaptopropyltrimethoxysilane, 3-isocyanatepropyltrimethoxysilane, and 3-isocyanatepropyltriethoxysilane are preferred. These silane coupling agents may be used alone or in combination of two or more.

[0189] In addition, the moisture-curable polyurethane resin may have both an isocyanate group and a hydrolyzable silyl group. The moisture-curable polyurethane resin having both an isocyanate group and a hydrolyzable silyl group is preferably manufactured by the following method: first, a moisture-curable polyurethane resin having an isocyanate group (raw polyurethane resin) is obtained by the above-mentioned method, and a silane coupling agent is further reacted with the raw polyurethane resin.

[0190] It should be noted that the details of the moisture-curable polyurethane resin with isocyanate group are as described above. As the silane coupling agent reacting with the raw material polyurethane resin, it is appropriate to select and use it from the silane coupling agents listed above, but from the viewpoint of reactivity with isocyanate group, it is preferred to use a silane coupling agent with amino or mercapto group. As a preferred specific example, N-(β-aminoethyl)-γ-aminopropyl trimethoxysilane, N-(β-aminoethyl)-γ-aminopropyl trimethyl dimethoxysilane, N-phenyl-γ-aminopropyl trimethoxysilane, γ-mercaptopropyl trimethoxysilane, γ-aminopropyl trimethoxysilane, 3-isocyanate propyl trimethoxysilane, etc. can be cited.

[0191] In addition, the moisture-curable resin may have a free radical polymerizable functional group. As the free radical polymerizable functional group that the moisture-curable resin may have, a group having an unsaturated double bond is preferred, and in particular, from the perspective of reactivity, a (meth)acryloyl group is more preferred. It should be noted that the moisture-curable resin having a free radical polymerizable functional group is not included in the above-mentioned free radical polymerizable compound and is treated as a moisture-curable resin (B).

[0192] The moisture-curable resin (B) may be appropriately selected from the above-mentioned various resins and used alone or in combination of two or more.

[0193] The weight average molecular weight of the moisture-curable resin (B) is preferably 7500 to 24000. By making the weight average molecular weight within the above range, it is easy to make the storage modulus (G') at 25°C and tanδ at 75°C of the optical moisture-curable resin composition within the specified range to improve the initial adhesion. In addition, by setting it below the above upper limit, it is easy to make the final adhesion good. From these viewpoints, the weight average molecular weight of the moisture-curable resin (B) is more preferably 7800 or more, further preferably 10000 or more, and further preferably 11500 or more. In addition, it is more preferably 20000 or less, more preferably 16000 or less, and further more preferably 15000 or less.

[0194] In addition, in this specification, the said weight average molecular weight is the value calculated|required by polystyrene conversion by gel permeation chromatography (GPC).

[0195] The moisture-curable resin may be chain-extended in order to adjust the weight average molecular weight to a certain value or more as described above.

[0196] For example, in the moisture-curable polyurethane resin, a polyurethane resin having an isocyanate group obtained by reacting a polyol compound with a polyisocyanate compound having two or more isocyanate groups in one molecule (hereinafter, also referred to as a "raw polyurethane resin") can be further reacted with a chain extender. In this case, the amount of the chain extender used can be appropriately adjusted so that the chain extender does not react with all the isocyanate groups of the raw polyurethane resin, thereby leaving isocyanate groups in the moisture-curable polyurethane resin. In addition, the chain extender that has reacted with the raw polyurethane resin can be further reacted with the raw polyurethane resin.

[0197] The chain extender used in the moisture-curable polyurethane resin is preferably a polyol compound. The details of the polyol compound are as described above. In addition, the polyol compound used as the chain extender can be a polyol compound of the same type as the polyol compound used to synthesize the raw material polyurethane resin. Therefore, if the polyol compound used to synthesize the raw material polyurethane resin is a polycarbonate polyol, the chain extender can also be a polycarbonate polyol.

[0198] The amount of the chain extender used is, for example, 5 to 40 parts by mass, preferably 10 to 35 parts by mass, and more preferably 15 to 30 parts by mass, based on 100 parts by mass of the total amount of the raw material polyurethane resin and the chain extender.

[0199] In the optical moisture curable resin composition, the mass ratio (B / A) of the moisture curable resin (B) to the radical polymerizable compound (A) is preferably 30 / 70 to 90 / 10, more preferably 40 / 60 to 80 / 20, and further preferably 50 / 50 to 70 / 30. By making the mass ratio within these ranges, the optical moisture curable resin composition can be imparted with light curing properties and moisture curing properties in a well-balanced manner, and both the initial adhesive strength and the final adhesive strength can be easily adjusted to the desired range.

[0200] The optical moisture curable resin composition may contain resin components other than the radical polymerizable compound (A) and the moisture curable resin (B) as resin components within a range that does not impair the effects of the present invention, and may contain, for example, resin components such as thermoplastic resins that are not curable (for example, acrylic resins, polyurethane resins, etc.), thermosetting resins, etc. The proportion of the resin components other than the radical polymerizable compound (A) and the moisture curable polyurethane resin (B) relative to 100 parts by mass of the total amount of the radical polymerizable compound (A) and the moisture curable polyurethane resin (B) is, for example, 50 parts by mass or less, preferably 30 parts by mass or less, and more preferably 10 parts by mass or less.

[0201] [Photopolymerization initiator (C)]

[0202] The optical moisture curable resin composition of the present invention contains a photopolymerization initiator. The optical moisture curable resin composition is appropriately provided with photocurability by containing a photopolymerization initiator.

[0203] Examples of the photopolymerization initiator include benzophenone compounds, acetophenone compounds, alkylphenone photopolymerization initiators, acylphosphine oxide compounds, titanocene compounds, oxime ester compounds, benzoin ether compounds, and thioxanthone.

[0204] Examples of commercially available photopolymerization initiators include IRGACURE 184, IRGACURE 369, IRGACURE 379, IRGACURE 379EG, IRGACURE 651, IRGACURE 784, IRGACURE 819, IRGACURE 907, IRGACURE 2959, IRGACURE OXE01, and IRGACURE TPO (all manufactured by BASF), benzoin methyl ether, benzoin ethyl ether, and benzoin isopropyl ether (all manufactured by Tokyo Chemical Industry Co., Ltd.).

[0205] The content of the photopolymerization initiator in the optical moisture curable resin composition is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the radical polymerizable compound (A). By making the content of the photopolymerization initiator within these ranges, the obtained optical moisture curable resin composition becomes a composition with excellent photocurability and storage stability. In addition, by setting it within the above range, the photo radical polymerizable compound is appropriately cured, and it is easy to make the adhesive force good.

[0206] [Filling agent (D)]

[0207] The optical moisture curable resin composition of the present invention may contain a filler (D). By containing a filler (D), the optical moisture curable resin composition of the present invention becomes a composition having suitable thixotropy and can fully maintain the shape after coating. As a filler, a particulate substance can be used.

[0208] As filler (D), inorganic filler is preferred, for example, silicon dioxide, talc, titanium oxide, zinc oxide, calcium carbonate, etc. can be cited. Among them, silicon dioxide is preferred from the aspect of excellent ultraviolet transmittance of the obtained light moisture curing resin composition. In addition, filler (D) can be subjected to hydrophobic surface treatment such as silylation treatment, alkylation treatment, epoxidation treatment, etc.

[0209] The filler (D) may be used alone or in combination of two or more.

[0210] The content of the filler (D) is preferably 1 to 25 parts by mass, more preferably 2 to 20 parts by mass, and even more preferably 3 to 15 parts by mass, relative to 100 parts by mass of the total amount of the radical polymerizable compound (A) and the moisture curable polyurethane resin (B).

[0211] (Moisture curing catalyst)

[0212] The optical moisture curable resin composition may contain a moisture curing accelerating catalyst for accelerating the moisture curing reaction of the moisture curable resin (B). By using a moisture curing accelerating catalyst, the optical moisture curable resin composition becomes a composition with better moisture curability and easily improves the adhesive force.

[0213] Specific examples of moisture curing accelerating catalysts include amine compounds, metal catalysts, etc. Examples of amine compounds include compounds having a morpholine skeleton such as di(methylmorpholino)diethyl ether, 4-morpholinopropylmorpholine, and 2,2'-dimorpholinodiethyl ether, dimethylamino group-containing amine compounds having two dimethylamino groups such as bis(2-dimethylaminoethyl)ether and 1,2-bis(dimethylamino)ethane, triethylamine, 1,4-diazabicyclo[2.2.2]octane, and 2,6,7-trimethyl-1,4-diazabicyclo[2.2.2]octane.

[0214] Examples of the metal catalyst include tin compounds such as di-n-butyltin dilaurate, di-n-butyltin diacetate, and tin octylate; zinc compounds such as zinc octylate and zinc naphthenate; and other metal compounds such as zirconium tetraacetylacetonate, copper naphthenate, and cobalt naphthenate.

[0215] The content of the moisture curing accelerating catalyst is preferably 0.01 to 8 parts by mass, more preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the moisture curable polyurethane resin (B). By making the content of the moisture curing accelerating catalyst within the above range, the storage stability of the optical moisture curable resin composition will not be deteriorated, and the effect of promoting the moisture curing reaction becomes excellent.

[0216] (Colorant)

[0217] The light moisture curable resin composition of the present invention may contain a colorant. Examples of the colorant include iron oxide, titanium black, aniline black, cyanine black, fullerene, carbon black, resin-coated carbon black, and the like. The light moisture curable resin composition contains a colorant, and the light shielding property and the like are also improved. Among these colorants, titanium black is preferred. Titanium black has the property of fully shielding light of wavelengths in the visible light region and transmitting light of wavelengths near the ultraviolet region, and thus can prevent the light curing property of the light moisture curable resin composition from being reduced.

[0218] The content of the colorant in the optical moisture curable resin composition is preferably 0.05 to 8 parts by mass, more preferably 0.1 to 2 parts by mass, relative to 100 parts by mass of the total amount of the free radical polymerizable compound (A) and the moisture curable polyurethane resin (B). By making the content of the colorant within these ranges, the adhesion of the optical moisture curable resin composition can be well maintained and appropriate light shielding properties can be imparted.

[0219] The optical moisture curing resin composition may contain other additives such as coupling agents, wax particles, ionic liquids, foamed particles, expanded particles, reactive diluents, etc. in addition to the components described above. It should be noted that the coupling agent includes silane coupling agents, titanate coupling agents, zirconate coupling agents, etc. Among these coupling agents, silane coupling agents are preferred.

[0220] The optical moisture curable resin composition may be diluted with a solvent as needed. When the optical moisture curable resin composition is diluted with a solvent, the mass parts of the optical moisture curable resin composition are based on the solid content, that is, the mass parts excluding the solvent.

[0221] As a method for producing the optical moisture curable resin composition of the present invention, there can be mentioned a method of mixing a radical polymerizable compound (A), a moisture curable resin (B), and a photopolymerization initiator (C), and other additives such as a filler, a moisture curing accelerator, and a colorant as required using a mixer, etc. Examples of the mixer include a homogenizer, a homomixer, a universal mixer, a planetary mixer, a planetary stirring device, a kneader, and a three-roller.

[0222] In addition, as described above, the molecular weight of a moisture-curable resin such as a moisture-curable polyurethane resin may be increased by using a chain extender. In this case, for example, a raw material resin such as a raw polyurethane resin may be reacted with a chain extender in advance to obtain a moisture-curable resin (B), and then other raw materials such as a free radical polymerizable compound (A) may be mixed as described above.

[0223] Alternatively, the raw material resin, the chain extender, and the radical polymerizable compound (A) may be mixed, and the mixture may be heated as required, so that the chain extender and the raw material resin react, thereby synthesizing the moisture-curable resin (B). In this case, a mixture of the moisture-curable resin (B) and the radical polymerizable compound (A) is obtained, and therefore, a photopolymerization initiator (C) and other additives may be added to the mixture as required, thereby obtaining an optical moisture-curable resin composition.

[0224] <Method of using the optical moisture curable resin composition>

[0225] The optical moisture curable resin composition of the present invention is a composition that can be cured and used as a cured product. Specifically, the optical moisture curable resin composition of the present invention can be first photocured by irradiation with light to form, for example, a B-stage state (semi-cured state), and then cured by moisture to fully cure.

[0226] Here, when the optical moisture curable resin composition is arranged between adherends so as to bond the adherends, it can be applied to one adherend, then photocured by light irradiation to form, for example, a B-stage state, and another adherend is superimposed on the optical moisture curable resin composition in the photocured state, and the adherends are temporarily bonded by a moderate adhesive force (initial adhesive force). Then, for the optical moisture curable resin composition in the B-stage state, the moisture curable polyurethane resin is cured by moisture, thereby being fully cured, and the superimposed adherends are formally bonded via the optical moisture curable resin composition and bonded with sufficient adhesive force.

[0227] The application of the optical moisture curable resin composition to the adherend can be performed by, for example, a dispenser, without particular limitation. The light irradiated during photocuring is not particularly limited as long as it is light for curing the radical polymerizable compound, but ultraviolet rays are preferred. In addition, when the optical moisture curable resin composition is fully cured by moisture after photocuring, it can be placed in the atmosphere for a predetermined time.

[0228] The application of the optical moisture curable resin composition to the adherend is not particularly limited, and can be carried out at around room temperature, specifically, at a temperature of about 10 to 35° C. Since the optical moisture curable resin composition of the present invention has a viscosity at 25° C. within the above-mentioned prescribed range, it can be easily applied even when applied at around room temperature, and liquid dripping does not occur.

[0229] Moreover, since the optical moisture curable resin composition of the present invention exhibits an initial adhesive force of a certain value or more immediately after light irradiation, temporary bonding can be performed immediately after photocuring, and workability becomes good.

[0230] The optical moisture curable resin composition of the present invention is preferably used as an adhesive for electronic components. That is, the present invention also provides an adhesive for electronic components formed from the optical moisture curable resin composition.

[0231] Therefore, the adherend is preferably various electronic components constituting electronic devices. Examples of the various electronic components constituting electronic devices include various electronic components provided in display elements, substrates on which electronic components are mounted, semiconductor chips, and the like.

[0232] In addition, the material of the adherend can be any material of metal, glass, plastic, etc. In addition, the shape of the adherend is not particularly limited, and for example, a film, sheet, plate, panel, disk, rod (rod-like body), box, shell, etc. can be cited.

[0233] As described above, the optical moisture curable resin composition of the present invention is preferably used to join electronic components constituting electronic devices. In addition, the optical moisture curable resin composition of the present invention is also preferably used to join electronic components to other components. Through these structures, the electronic component has a cured body of the present invention.

[0234] In addition, the optical moisture curable resin composition of the present invention is used in the interior of an electronic device, for example, to bond substrates to each other to obtain an assembly. The assembly obtained by such operation comprises a first substrate, a second substrate, and a cured product of the present invention, and at least a portion of the first substrate is bonded to at least a portion of the second substrate via the cured product. It should be noted that the first substrate and the second substrate are preferably each mounted with at least one electronic component.

[0235] In addition, the light moisture curing type resin composition of the present invention is preferably used in narrow frame applications. For example, in various display element devices such as display devices for mobile phones such as smart phones, an adhesive is applied to a substrate in a narrow square frame shape (i.e., a narrow frame), and a display panel, a touch panel, etc. are assembled by the adhesive. As the adhesive, the light moisture curing type resin composition of the present invention can be used. In addition, the light moisture curing type resin composition of the present invention is preferably used in semiconductor chip applications. The light moisture curing type resin composition of the present invention is used in the application of semiconductor chips, for example, to join semiconductor chips to each other.

[0236] Example

[0237] The present invention will be described in more detail using examples, but the present invention is not limited to these examples.

[0238] Various physical properties were measured and evaluated as follows.

[0239] (Weight average molecular weight)

[0240] The weight average molecular weight of the moisture curable resin (B) in each embodiment and comparative example was measured by gel permeation chromatography (GPC) and obtained by polystyrene conversion. Shodex KF-806L (Showa Denko Co., Ltd.) was used as a column for GPC measurement. In addition, tetrahydrofuran (THF) was used as a solvent and mobile phase. In addition, as the measurement conditions of GPC, the flow rate was 1.0 ml / min and the measurement temperature was 40 ° C.

[0241] It should be noted that in each example and comparative example, the weight average molecular weight is measured using a mixture of a radical polymerizable compound and a moisture curable resin (B) as a sample. In the mixture, a peak of the radical polymerizable compound appears on the low molecular weight side, and a peak of the moisture curable resin (B) appears on the high molecular weight side. Therefore, the weight average molecular weight of the moisture curable resin (B) can be obtained from the peak on the high molecular weight side.

[0242] (Viscosity at 25℃)

[0243] The viscosity at 25° C. was measured under the conditions of 5.0 rpm and 25° C. using a cone-plate viscometer (trade name TVE-35, manufactured by Toki Sangyo Co., Ltd.).

[0244] (Storage modulus (G') at 25°C and tanδ at 75°C)

[0245] As a dynamic viscoelasticity measuring device, a product name "DVA-200" manufactured by ITECH Instruments Co., Ltd. was used. As a viscoelasticity measuring fixture, a shear test fixture was used. A light moisture curable resin composition of 0.6 mm × 6 mm × 9 mm was set on the viscoelasticity measuring fixture. For a 1000 mJ / cm 2 The sample photocured by irradiation with ultraviolet light having a wavelength of 405 nm was measured by the method described in the manual.

[0246] (Inside-outside ratio a / b)

[0247] The inside-outside ratio a / b was measured using the method described in the specification. It should be noted that, as the aluminum substrate and glass plate, an aluminum alloy "A6063S" with a size of 2 mm × 25 mm × 60 mm and a glass plate with a smooth surface that had been ultrasonically cleaned for 5 minutes were used, respectively. The moisture-curing resin composition was applied at room temperature (25°C) using "SHOTMASTER300SX" manufactured by Musashi Engineering Co., Ltd. as a dispensing device, and was applied to the aluminum substrate in a straight line with a width of 1.0±0.1 mm, a length of 25 mm, and a thickness of 0.4±0.1 mm. Next, the applied optical moisture-curing resin composition was irradiated with a linear LED irradiator (manufactured by HOYA Corporation, 1000 mW) at a rate of 1000 mJ / cm 2 Ultraviolet rays with a wavelength of 405 nm were irradiated. The glass plate was pressed against the aluminum substrate using a weight as a weight, and the widths a1 and b1 were measured 5 minutes after the weight was removed. The widths a1 and b1 after pressing were measured by observing the pressing surface from the glass plate side using a microscope.

[0248] (Initial Adhesion)

[0249] like Figure 2 As shown in (a) and (b), the optical moisture curable resin composition 20 was applied to the aluminum substrate 21 at room temperature (25°C) using the above-mentioned dispensing device in a manner of 1.0±0.1 mm in width, 25 mm in length, and 0.4±0.1 mm in thickness. Then, a linear LED irradiator (manufactured by HOYA Corporation, 1000 mW) was used to irradiate the aluminum substrate 21 at 1000 mJ / cm 2 Then, a glass plate 22 was bonded to the aluminum substrate 21 via the photocured optical moisture curable resin composition 20, and the coated area was pressed at 0.08 MPa for 120 seconds using a weight to obtain a sample 23 for evaluating adhesion.

[0250] Then, in an atmosphere of 25°C, the aluminum substrate 21 and the glass plate 22 were stretched at a speed of 10 mm / min along the shear direction S using a tensile tester ("tensile compression tester SVZ-50NB", manufactured by Imada Manufacturing Co., Ltd.), and the maximum stress when peeling off was measured as the initial bonding strength. It should be noted that the test was performed within 150 seconds from the end of photocuring to the start of the tensile test. The initial bonding strength was evaluated according to the following evaluation criteria.

[0251] A: 0.4MPa or more

[0252] B: 0.25MPa or more and less than 0.4MPa

[0253] C: less than 0.25MPa

[0254] (Final bonding strength)

[0255] As with the initial adhesive strength, a glass plate was bonded to the aluminum substrate via a light-cured optical moisture-curable resin composition. Then, the sample was placed at 25°C and 50 RH% for 24 hours for moisture curing to obtain a sample for evaluating adhesion. Using the sample for evaluating adhesion, the sample was stretched in the shear direction in the same manner as the method for measuring the initial adhesive strength, and the maximum stress when the aluminum substrate and the glass plate were peeled off was measured as the final adhesive strength.

[0256] A: 3.5MPa or more

[0257] B: 2.0MPa or more and less than 3.5MPa

[0258] C: less than 2.0MPa

[0259] The polyurethane resin raw material used in each of the Examples and Comparative Examples was produced by the following method.

[0260] [Synthesis example 1]

[0261] (PC polyurethane resin raw material)

[0262] 100 parts by mass of polycarbonate diol (a compound represented by formula (1), 90 mol% of R is 3-methylpentylene and 10 mol% is 1,6-hexylene, manufactured by Kuraray Co., Ltd., trade name "Kuraraypolyol C-1090") as a polyol compound and 0.01 parts by mass of dibutyltin dilaurate were placed in a 500 mL separable flask. The mixture was stirred in a flask at 100° C. for 30 minutes under vacuum (below 20 mmHg). The mixture was then set to normal pressure, 50 parts by mass of diphenylmethane diisocyanate (manufactured by Nichisou Shoji Co., Ltd., trade name "Pure MDI") as a polyisocyanate compound was added, and the mixture was reacted by stirring at 80° C. for 3 hours to obtain a moisture-curable polyurethane resin (PC polyurethane resin raw material) having a polycarbonate skeleton and isocyanate groups at both ends. The weight average molecular weight of the obtained polyurethane resin raw material was 6700.

[0263] [Synthesis example 2]

[0264] (ET polyurethane resin raw material)

[0265] 100 parts by mass of polytetramethylene ether glycol (Mitsubishi Chemical Co., trade name "PTMG-3000") as a polyol compound and 0.01 parts by mass of dibutyltin dilaurate were placed in a 500 mL separable flask. Under vacuum (below 20 mmHg), the flask was stirred at 100 ° C for 30 minutes and mixed. Then it was set to normal pressure, 17.5 parts by mass of diphenylmethane diisocyanate (Nissou Shoji Co., trade name "Pure MDI") as a polyisocyanate compound was added, and stirred at 80 ° C for 3 hours to react to obtain a moisture-curable polyurethane resin (ET polyurethane resin raw material) having a polyether skeleton and an isocyanate group at both ends. The weight average molecular weight of the obtained polyurethane resin raw material is 3500.

[0266] [Example 1]

[0267] As described in Table 5, each raw material constituting 60 parts by mass of moisture-curable resin (PC-L25) was added to 40 parts by mass of acrylic acid (acryl) A. Acrylic acid A is a material obtained by mixing each compound at the mixing ratio described in Table 2. As a moisture-curable resin (PC-L25), a PC polyurethane resin raw material and a PC polyol were sequentially added to acrylic acid A at the mass ratio described in Table 3 to obtain a mixture. As PC polyol, the polycarbonate diol used in Synthesis Example 1 was used.

[0268] The obtained mixture was stirred at 50° C. to react part of the polyurethane resin raw material with the polyol to synthesize a moisture-curable polyurethane resin having an extended chain and residual isocyanate group, thereby obtaining a mixture of acrylic acid A (radical polymerizable compound) and moisture-curable polyurethane resin.

[0269] A photopolymerization initiator and a filler were added to the obtained mixture of acrylic acid A and moisture-curable polyurethane resin according to the compounding shown in Table 5, and the mixture was further mixed to obtain an optical moisture-curable resin composition. The viscosity at 25° C., the storage modulus (G') at 25° C., the tan δ at 75° C., the internal-external ratio a / b, the initial adhesive strength, and the final adhesive strength of the obtained optical moisture-curable resin composition were measured.

[0270] [Examples 2 to 4, 7, 8, Comparative Examples 1 and 2]

[0271] The same procedure as in Example 1 was carried out except that acrylic acid B was used instead of acrylic acid A and that moisture-curable resins described in Tables 3, 4, and 5 were used instead of the moisture-curable resin (PC-L25).

[0272] That is, the same method as in Example 1 was used except that acrylic acid B was used instead of acrylic acid A, and the mixing ratio and type of the polyurethane resin raw material and the polyol added to acrylic acid B were changed as described in Tables 3 and 4 to obtain a mixture of acrylic acid B and a moisture-curable polyurethane resin. It should be noted that the ET polyol in Table 4 is the polytetramethylene ether glycol used in Synthesis Example 2. In Comparative Example 1, only the polyurethane resin raw material was added to acrylic acid A without adding a polyol, and therefore the polyurethane resin raw material was used as a moisture-curable resin as it was.

[0273] [Examples 5, 9 to 11, Comparative Examples 3 to 5]

[0274] The same procedure as in Example 1 was carried out except that acrylic acid B to H were used instead of acrylic acid A. In addition, acrylic acid B to H were obtained by mixing the respective compounds at the blending ratios described in Table 2, respectively.

[0275] [Example 6]

[0276] The same procedures as in Example 5 were carried out except that a photopolymerization initiator, a filler, and a colorant were added to the obtained mixture of acrylic acid B and moisture-curable polyurethane resin according to the compounding in Table 5 and mixed to obtain an optical moisture-curable resin composition.

[0277] Components other than the moisture-curable polyurethane resin (B) used in each of the Examples and Comparative Examples are as shown in Table 1 below.

[0278] Table 1

[0279]

[0280] Acrylic acids A to H used in Examples and Comparative Examples are as follows.

[0281] Table 2

[0282]

[0283] The moisture-curable resins (B) used in the examples and comparative examples are shown in the following Table 3. As described above, in the moisture-curable resin (L0), the polyurethane resin raw material was used as the moisture-curable resin (B) as it is, and in the other moisture-curable resins, the reaction products of the following polyurethane resin raw materials and polyols were used as the moisture-curable resin (B).

[0284] Table 3

[0285]

[0286] Table 4

[0287]

[0288]

[0289] The optical moisture curable resin compositions of Examples 1 to 11 contain a radical polymerizable compound (A), a moisture curable resin (B), and a photopolymerization initiator (C), and the storage modulus (G') at 25°C and tan δ at 75°C are greater than or equal to the specified values, so the initial adhesive force is excellent. In contrast, in Comparative Examples 1 to 5, since at least one of the storage modulus (G') at 25°C and tan δ at 75°C is less than the specified value, the initial adhesive force cannot be improved.

Claims

1. An optical moisture curable resin composition comprising a radical polymerizable compound (A), a moisture curable resin (B), and a photopolymerization initiator (C), The optical moisture curable resin composition is irradiated with 1000 mJ / cm 2 In a state where the film is photocured by ultraviolet rays, the storage modulus (G') at 25°C when measured at 1 Hz by a dynamic viscoelasticity measuring device is 250 kPa or more, and the tan δ at 75°C is 1.0 or more.

2. The optical moisture curable resin composition according to claim 1, wherein the optical moisture curable resin composition is applied to an aluminum substrate with a line width of 1.0 mm and irradiated with 1000 mJ / cm 2 The glass plates were pressed at 0.08 MPa for 120 seconds under a state of photocuring by ultraviolet rays. At this time, if the average width of the bonding portion on the glass plate side is set to a and the average width of the bonding portion on the aluminum substrate side is set to b, a / b is 0.58 to 0.

99. 3 . The optical moisture-curable resin composition according to claim 1 , wherein the moisture-curable resin (B) comprises a moisture-curable polyurethane resin. 4 . 4 . The optical moisture curable resin composition according to claim 1 , wherein the weight average molecular weight of the moisture curable resin (B) is 7500 or more and 24000 or less. 5 . The optical moisture curable resin composition according to claim 1 , wherein the radically polymerizable compound (A) contains a monofunctional radically polymerizable compound. 6 . The optical moisture curable resin composition according to claim 5 , comprising 90 parts by mass or more of the monofunctional radical polymerizable compound based on 100 parts by mass of the radical polymerizable compound (A). 7 . The optical moisture curable resin composition according to claim 1 , further comprising a filler (D). 8 . An adhesive for electronic components, comprising the optical moisture curable resin composition according to claim 1 . 9 . A cured product, which is a cured product of the optical moisture curable resin composition according to claim 1 . 10 . An electronic component comprising the cured product according to claim 9 .