Efficient degreasing technology for sheepskin
The reaction of aminobiurea glyoxaldehyde condensate with collagen fibers increases the shrinkage temperature of the bare skin, solves the problem of degreasing temperature control, achieves efficient degreasing and improves leather performance, reduces the amount of degreasing agents and chromium powder, and promotes the clean production of leather .
Patent Information
- Application Number
- CN202410973360.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art causes leather loss due to improper temperature control during degreasing, and the amount of degreasing agent is large, resulting in high costs and environmental pollution, making it difficult to achieve complete degreasing.
The aminobisurea glyoxaldehyde condensate is used as the degreasing pretreatment agent to produce irreversible crosslinking by reacting with collagen fibers, which increases the shrinkage temperature of the bare skin, and degreasing under high temperature conditions to reduce the amount of degreasing agent.
It improves degreasing efficiency, reduces the amount of degreasing agent, reduces the amount of chromium powder, improves the performance and tensile strength of the leather, reduces the residual concentration of chromium in the waste liquid, and realizes clean leather production.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of leather processing, in particular to a sheepskin efficient degreasing technology. Background Art
[0002] Sheep skin is an important fabric for clothing and shoes. It is a raw material with a high fat content. Its fat content can be as high as 30% of the skin weight. At the same time, the solidification point of sheep fat is about 38-42℃. The optimal emulsification temperature of sheep skin is above 42℃, but the shrinkage temperature of bare skin is mostly below 45℃, which makes conventional degreasing and subsequent water washing mostly carried out at 38-40℃. Due to the limitation of reaction temperature, in order to achieve complete degreasing, the amount of degreasing agent is generally large, and some degreasing agents are used as high as 10% or even higher, which is not only costly, but also causes serious environmental problems. Further improvement is still needed. Summary of the invention
[0003] The object of the present invention is to provide a sheepskin efficient degreasing technology to solve the above-mentioned problems in the background technology. The aminobisurea glyoxal condensate obtained by the degreasing pretreatment agent preparation method of the present invention can increase the bare skin shrinkage temperature to 60-70°C. For fatty leather (such as sheepskin, etc.), it can be degreased in a degreasing bath above 45°C, which improves the degreasing efficiency and can reduce the amount of degreasing agent, which is beneficial to the clean production needs of leather. After being treated by the high-temperature degreasing and high-temperature degreasing leather making process of the present invention, the fat content of blue leather can be ≤3%.
[0004] To achieve the above object, the present invention provides the following technical solutions:
[0005] One of the technical solutions of the present invention is to provide a method for preparing a degreasing pretreatment agent, comprising the following steps:
[0006] The polyethylene polyamine and the urea donor are mixed and reacted, and then water is added and stirred to obtain an aminobisurea polymer aqueous solution, and then glyoxal is added and reacted twice to obtain the degreasing pretreatment agent.
[0007] Preferably, the polyethylene polyamine includes one or more of diethylenetriamine, triethylenetetramine and tetraethylenepentamine; and the urea group donor is thiourea and / or urea.
[0008] Preferably, the reaction temperature is 120-210° C. and the reaction time is 4-12 h.
[0009] Preferably, the mass concentration of the aminobisurea polymer aqueous solution is 50%; the molar ratio of the polyethylene polyamine, the urea donor and glyoxal is 1:2.01-2.2:0.5-4.0.
[0010] Preferably, the temperature of the secondary reaction is 30-80°C and the time is 4-12h.
[0011] The second technical solution of the present invention is to provide a degreasing pretreatment agent obtained according to the above preparation method.
[0012] The third technical solution of the present invention is to provide an application of the above-mentioned degreasing pretreatment agent in the high-temperature degreasing leather making process of sheepskin.
[0013] The fourth technical solution of the present invention is to provide a method for high-temperature degreasing and leather making of sheepskin, wherein the sheepskin is firstly degreased using the above-mentioned degreasing pretreatment agent, and then degreased at high temperature.
[0014] Preferably, the degreasing pretreatment comprises the following steps: mixing the sheepskin and the degreasing pretreatment agent in water, and soaking them to complete the degreasing pretreatment;
[0015] The high temperature degreasing comprises the following steps: adding nonionic degreasing agent SINOBEAMD50, water and leather material pretreated by degreasing into a rotary drum at 48-50°C, degreasing for 2 hours, and washing with water at 45-50°C to complete the high temperature degreasing.
[0016] Preferably, in the degreasing pretreatment step: the mass concentration of the degreasing pretreatment agent in the solution is 2-4%; the pH value of the soaking is 8.2-8.5, and the soaking time is 2-4h;
[0017] In the high-temperature degreasing step, the mass ratio of the water, the nonionic degreasing agent SINOBEAM D50 and the leather material after degreasing pretreatment is 100:2-4:100.
[0018] The beneficial technical effects of the present invention are as follows:
[0019] The degreasing pretreatment agent designed by the present invention combines well with collagen fibers, can react with skin fibers under the condition of pH=8.2-8.5 to produce irreversible crosslinking, so that the molecular configuration of collagen fibers is rigidified, and the framework structure formed by molecular association improves the stability of collagen to a certain extent, especially the molecular chain segments introduce aldehyde groups with covalent crosslinking with collagen fibers, which can stably improve the wet heat stability of collagen. After degreasing pretreatment, the shrinkage temperature of bare skin can be quickly increased to above 60-70°C, which creates the possibility of degreasing at a temperature above 48°C in the later stage, thereby achieving the purpose of efficient degreasing and thorough degreasing.
[0020] The aminobisurea glyoxal condensate obtained by the degreasing pretreatment agent preparation method of the present invention can increase the shrinkage temperature of bare leather to 60-70°C, and can avoid the loss of leather such as scalding caused by improper temperature control during the degreasing process. For fatty leather (such as sheepskin, etc.), it can be degreased in a degreasing bath above 45°C, which improves the degreasing efficiency and can reduce the amount of degreasing agent, which is beneficial to the clean production demand of leather. After being treated by the high-temperature degreasing and high-temperature degreasing leather making process of the present invention, the fat content of blue leather can be made ≤3%. The bare leather pretreated by degreasing can reduce the amount of chromium powder, improve the absorption rate of chrome tanning agent, and the residual Cr2O3 concentration of waste liquid chromium reaches below 0.3g / L, and even if the leather is treated with only 4% of the chromium powder equivalent to the leather weight, the shrinkage temperature of the obtained blue leather can reach above 95°C, while improving the leather performance, and the leather embryo tensile strength reaches 20-35N / mm 2 . DETAILED DESCRIPTION
[0021] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.
[0022] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0023] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.
[0024] The words “include,” “including,” “have,” “contain,” etc. used in the present invention are open-ended terms, meaning including but not limited to.
[0025] Unless otherwise specified, "overnight" in the present invention is calculated as 12 hours.
[0026] The "normal temperature" in the present invention is 22°C unless otherwise specified.
[0027] Unless otherwise specified, the "liquid ratio" in the present invention is calculated based on the mass ratio of the liquid phase component in the drum to the leather material.
[0028] The percentages of the various raw materials described in the following embodiments and comparative examples of the present invention are all calculated based on the mass percentage of the various raw materials to the leather material.
[0029] The raw material skins used in the following examples and comparative examples of the present invention were weighed after fully removing the salt, which was used as the basis for measurement.
[0030] All raw materials used in the following examples and comparative examples of the present invention are commercially available products.
[0031] Example 1
[0032] Preparation of degreasing pretreatment agent:
[0033] Dissolve urea (2.02 mol) in diethylenetriamine (1 mol) kept at 80°C, keep the reaction system completely sealed, continue to heat up to 150°C, react for 6 hours, then cool the reaction system to 120°C, carefully add 90°C hot water and stir quickly to fully dissolve to obtain a light yellow aminobisurea polymer aqueous solution with a mass concentration of 50%, then add 4.0 mol of glyoxal, and react for 4 hours at 40°C to obtain a degreasing pretreatment agent.
[0034] Preparation of blue leather for sheepskin uppers:
[0035] (1) Pre-soaking: At 20-22°C, water and raw hides are put into a drum in a mass ratio of 300%, 0.1% fungicide XJ150 and 6% salt are added, the drum is rotated for 5 minutes, and then left to stand overnight, and then rotated for 5 minutes every hour thereafter, for a total of 6 hours, and then the solution in the drum is discharged.
[0036] (2) Water washing: Add water equivalent to 300% of the leather mass into the drum again, rotate for 10 minutes, and then drain the solution in the drum.
[0037] (3) Re-washing: Add water equivalent to 300% of the leather mass into the drum again, rotate for 10 minutes, and then drain the solution in the drum.
[0038] (4) Main immersion: The main immersion liquid is prepared according to the following mass percentages: 0.15% of immersion agent SINOBEAM SA, 0.15% of bactericide SINOBEAM XJ150, 0.3% of degreasing agent SINOBEAM DG, and the balance is water.
[0039] Add the main soaking liquid equivalent to 300% of the leather mass into the drum, rotate for 20 minutes, let it stand for 40 minutes, and then rotate for 3 minutes every hour, for a total of 18 hours; among them, add 0.15% of the fungicide SINOBEAM XJ150 after 6 hours of circulation. After the cycle is completed, rotate for 10 minutes, and then drain the liquid and take out the leather.
[0040] (5) Meat removal: Use a meat remover to remove the meat.
[0041] (6) Lime coating and hair pushing: prepare 35g / L alkali sulfide solution and mix it with corn starch to make a paste. Apply it evenly on the leather surface, let it stand for 4 hours, and then push the leather by hand.
[0042] (7) Liming:
[0043] At 22°C, add water equivalent to 100% of the mass of the leather into the drum, add 0.1% sodium hydrosulfide and 1.5% liming agent SINOBEAM LM, then rotate for 40 minutes, stop for 30 minutes, then add 0.3% alkali sulfide, 0.2% sodium hydrosulfide, 0.2% lime powder, rotate for 10 minutes, stop for 20 minutes, repeat 5 times (total time 150 minutes), add 0.6% CR and 0.2% lime powder, rotate for 10 minutes, stop for 20 minutes, repeat 4 times (total time 120 minutes), add water until the mass ratio of liquid to leather is 250%, continue to rotate for 30 minutes, stop for 30 minutes, rotate for 10 minutes, stop the drum, then cycle 6 times in a way of rotating for 3 minutes per hour, and drain the liquid.
[0044] (8) Deliming and softening: At 26-28°C, add water equivalent to 100% of the leather mass into a rotating drum, then add 0.4% of deliming agent SINOBEAM DL22 and 0.4% of ammonium sulfate, rotate for 20 minutes, then add 0.3% of ammonium sulfate, rotate for 40 minutes, then add 0.3% of softening enzyme NS, rotate for 15 minutes, control the liquid at pH = 6.5-7.5, rinse twice with normal temperature water, and drain.
[0045] (9) Degreasing pretreatment: At 30°C, add water equivalent to 100% of the mass of the leather into a rotating drum, then add 4% of the aminobisurea pretreatment agent in this embodiment (calculated as the mass percentage of the aminobisurea pretreatment agent to the leather), and add soda ash to adjust the pH to 8.2. Rotate for 120 minutes, wash with water at room temperature, and drain.
[0046] (10) Degreasing: At 48°C, add water equivalent to 100% of the leather mass into a rotating drum, then add 1.5% of SINOBEAMAD, a degreasing agent, and rotate for 90 minutes. Drain the liquid, then wash it twice with 45°C water (liquid ratio 200%), each time for 20 minutes, and then wash it twice with 22°C water (liquid ratio 300%), each time for 10 minutes, and drain the liquid.
[0047] (11) Pickling: At room temperature, add water equivalent to 100% of the hide mass into a rotating drum, then add 2% sodium formate, 2% salt, and 1.0% sulfuric acid, rotate for 90 minutes, and drain.
[0048] (12) Tanning: Chrome powder 5.5%, rotate for 3 hours, check
[0049] MgO 0.3% rotation for 60 minutes
[0050] Chromium absorption accelerator 0.3% rotation for 60 minutes
[0051] Water 200%, internal temperature 40°C, rotate for 5 hours, take out of the drum and let it stand to obtain blue skin.
[0052] The free fat content of the blue leather was 1.87%, the shrinkage temperature was 101.3℃, and the tensile strength was 28.27N / mm. 2 .
[0053] Example 2
[0054] Preparation of degreasing pretreatment agent:
[0055] 0.6 mol of diethylenetriamine, 0.3 mol of triethylenetetramine and 0.1 mol of tetraethylenepentamine were mixed and kept warm at 80°C, then 1.01 mol of thiourea and 1.1 mol of urea were dissolved therein, the reaction system was kept completely sealed, the temperature was continued to be raised to 185°C, and after reacting for 4 hours, the reaction system was cooled to 120°C, 90°C hot water was carefully added and stirred rapidly to fully dissolve, and a light yellow aminobisurea polymer aqueous solution with a mass concentration of 50% was obtained, and then 2.2 mol of glyoxal was added, and a secondary reaction was carried out at 40°C for 12 hours to obtain a degreasing pretreatment agent.
[0056] Preparation of blue leather for sheepskin clothing:
[0057] (1) Pre-soaking: At 20-22°C, water and raw hides are put into a drum in a mass ratio of 300%, 0.1% fungicide XJ150 and 6% salt are added, the drum is rotated for 5 minutes, and then left to stand overnight, and then rotated for 5 minutes every hour thereafter, for a total of 6 hours, and then the solution in the drum is discharged.
[0058] (2) Water washing: Add water equivalent to 300% of the leather mass into the drum again, rotate for 10 minutes, and then drain the solution in the drum.
[0059] (3) Re-washing: Add water equivalent to 300% of the leather mass into the drum again, rotate for 10 minutes, and then drain the solution in the drum.
[0060] (4) Main immersion: The main immersion liquid is prepared according to the following mass percentages: 0.15% immersion agent SINOBEAM SA, 0.15% bactericide SINOBEAM XJ150, 0.5% degreasing agent SINOBEAM DG, and the balance is water.
[0061] Add the main soaking liquid equivalent to 300% of the leather mass into the drum, rotate for 20 minutes, let it stand for 40 minutes, and then rotate for 3 minutes every hour, for a total of 18 hours; among them, add 0.15% of the fungicide SINOBEAM XJ150 after 6 hours of circulation. After the cycle is completed, rotate for 10 minutes, and then drain the liquid and take out the leather.
[0062] (5) Meat removal: Use a meat remover to remove the meat.
[0063] (6) Lime coating and hair removal: Prepare 120g / L alkali sulfide solution and mix it with corn starch to make a paste. Apply it evenly on the leather surface, let it stand for 2 hours, and remove the hair manually.
[0064] (7) Liming:
[0065] At 22°C, add water equivalent to 100% of the mass of the leather into the drum, add 0.4% sodium hydrosulfide and 1.2% liming agent SINOBEAM LM, then rotate for 40 minutes, stop for 30 minutes, then add 0.5% sodium sulfide, 0.2% sodium hydrosulfide, 1.0% lime powder, rotate for 10 minutes, stop for 20 minutes, repeat 5 times (total time 150 minutes), add 0.3% CR and 1.0% lime powder, rotate for 10 minutes, stop for 20 minutes, repeat 4 times (total time 120 minutes), add water until the liquid ratio to the mass ratio of the leather is 250%, continue to rotate for 30 minutes, stop for 30 minutes, rotate for 10 minutes, stop the drum, then cycle 6 times in a way of rotating for 3 minutes per hour, and drain the liquid.
[0066] (8) Deliming and softening: At 26-28°C, add water equivalent to 100% of the leather mass into a rotating drum, then add 0.4% of deliming agent SINOBEAM DL22 and 0.6% of ammonium sulfate, rotate for 20 minutes, then add 0.6% of ammonium sulfate, rotate for 40 minutes, then add 0.4% of softening enzyme NS, rotate for 40 minutes, control the liquid at pH = 6.5-7.5, rinse twice with room temperature water, and drain.
[0067] (9) Degreasing pretreatment: At 30°C, add water equivalent to 100% of the leather mass into a rotating drum, then add 3% of the aminobisurea pretreatment agent in this example, and add soda ash to adjust the pH to 8.3. Rotate for 120 minutes, wash with water at room temperature, and drain.
[0068] (10) Degreasing: At 50°C, add water equivalent to 100% of the leather mass into a drum, then add 2% of the degreasing agent SINOBEAM AD, rotate for 90 minutes, drain the liquid, and then wash it twice with 50°C water (liquid ratio 200%), each time for 20 minutes, and then wash it twice with 22°C water (liquid ratio 300%), each time for 10 minutes, and drain the liquid.
[0069] (11) Pickling: At room temperature, add water equivalent to 100% of the hide mass into a rotating drum, then add 2% sodium formate, 2% salt, and 1.4% sulfuric acid, rotate for 90 minutes, and drain.
[0070] (12) Tanning: Chrome powder 4.5%, rotate for 3 hours, check
[0071] MgO 0.3% rotation for 60 minutes
[0072] Chromium absorption accelerator 0.3% rotation for 60 minutes
[0073] Water 200%, internal temperature 40°C, rotate for 5 hours, take out of the drum and let it stand to obtain blue skin.
[0074] The free fat content of the blue leather was 1.13%, the shrinkage temperature was 95.7℃, and the tensile strength was 21.08N / mm. 2 . .
[0075] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing a degreasing pretreatment agent, It is characterized in that The following steps are involved: The polyethylene polyamine and the urea donor are mixed and reacted, and then water is added and stirred to obtain an aminobisurea polymer aqueous solution, and then glyoxal is added and reacted twice to obtain the degreasing pretreatment agent.
2. The preparation method according to claim 1, It is characterized in that The polyethylene polyamine includes one or more of diethylenetriamine, triethylenetetramine and tetraethylenepentamine; and the urea group donor is thiourea and / or urea.
3. The preparation method according to claim 1, It is characterized in that The reaction temperature is 120-210° C. and the reaction time is 4-12 hours.
4. The preparation method according to claim 1, It is characterized in that The mass concentration of the aminobisurea polymer aqueous solution is 50%; the molar ratio of the polyethylene polyamine, the urea donor and glyoxal is 1:2.01-2.2:0.5-4.
0.
5. The preparation method according to claim 1, It is characterized in that The temperature of the secondary reaction is 30-80°C and the time is 4-12h.
6. A degreasing pretreatment agent obtained according to the preparation method according to any one of claims 1 to 5.
7. Use of the degreasing pretreatment agent according to claim 6 in a high-temperature degreasing leather making process for sheepskin.
8. A method for high temperature degreasing of sheepskin leather, It is characterized in that The sheepskin is firstly subjected to degreasing pretreatment using the degreasing pretreatment agent as claimed in claim 6, and then subjected to high temperature degreasing.
9. The method according to claim 8, It is characterized in that The degreasing pretreatment comprises the following steps: mixing the sheepskin and the degreasing pretreatment agent in water, soaking the sheepskin and the degreasing pretreatment agent in water, and completing the degreasing pretreatment; The high temperature degreasing comprises the following steps: adding nonionic degreasing agent SINOBEAM D50, water and leather material pretreated by degreasing into a rotary drum at 48-50° C., degreasing for 2 hours, and washing with water at 45-50° C. to complete the high temperature degreasing.
10. The method according to claim 9, It is characterized in that In the degreasing pretreatment step: the mass concentration of the degreasing pretreatment agent in the solution is 2-4%; the pH value of the soaking is 8.2-8.5, and the soaking time is 2-4h; In the high-temperature degreasing step, the mass ratio of the water, the nonionic degreasing agent SINOBEAM D50 and the leather material after degreasing pretreatment is 100:2-4:100.