Epoxy resin composition, hydrogen storage bottle and preparation method
By adding reactive toughener and halogen-free flame retardant to the epoxy resin system of the hydrogen storage cylinder, the problem of poor flame retardant performance in the prior art is solved, and the toughness and flame retardant performance of the hydrogen storage cylinder are improved, ensuring that The product is safe and aesthetically pleasing and suitable for wet winding forming process.
Patent Information
- Application Number
- CN202410918728.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
AI Technical Summary
The flame retardant properties of existing epoxy resins for hydrogen storage cylinders are poor, and traditional modification methods affect toughness and heat resistance, resulting in safety hazards and unfavorable market sales.
By adding a variety of reactive toughening agents and halogen-free flame retardant to the epoxy resin system, an epoxy resin composition with high toughness, high flame retardancy and aesthetics is prepared, which is suitable for wet winding molding process.
It achieves the improvement of high toughness, heat resistance and flame retardant performance of hydrogen storage cylinders, ensures the safety of the product under high temperature and combustion conditions, and maintains a beautiful appearance, suitable for market sales.
Smart Images

Figure BDA0004935969920000131 
Figure BDA0004935969920000141 
Figure BDA0004935969920000151
Abstract
Description
Technical Field
[0001] The invention belongs to the field of composite materials, and specifically relates to an epoxy resin composition, a hydrogen storage bottle and a preparation method. Background Art
[0002] With the increasing demand for energy transformation and the rapid development of hydrogen energy technology in my country, hydrogen storage technology has received extensive attention as an important part of the hydrogen energy industry chain. At present, the research on pressure gas cylinders in China is focused on Type IV hydrogen storage cylinders. Type IV hydrogen storage cylinders are mainly formed by winding carbon fibers impregnated with epoxy resin glue and then wound around a plastic liner. In actual application scenarios, not only during the inflation process, the gas cylinders face instantaneous high pressure, but also due to accidents during use, there are great safety hazards. Therefore, in order to ensure the safety of the hydrogen storage system, it is necessary to develop a flame-retardant and high-toughness resin system for the molding of hydrogen storage bottles.
[0003] At present, most hydrogen storage cylinders on the market use epoxy resin systems. The molecular structure of epoxy resin contains a large number of benzene rings and ether bonds. These structures make epoxy resin have excellent mechanical properties, chemical corrosion resistance and electrical insulation, but also lead to poor toughness and flame retardancy of epoxy resin. Traditional methods for flame retardant modification of epoxy resin systems mostly use inorganic fillers or brominated epoxy modification, which has the problem of large addition amount, affecting the heat resistance of the resin system, greatly reducing the toughness of the resin system, affecting the wettability of the resin and fiber or easily generating irritating and toxic gases to pollute the environment during use, and the surface of the molded cylinder is yellow and cracked, which is not conducive to market sales.
[0004] For example, Chinese patent document with publication number CN117659623A discloses a method for preparing a modified epoxy resin, which increases the toughness of the resin by adding rubber particles and using interpenetrating polymer network technology. The rubber particles form microphase separation during the hardening process, which helps to absorb stress and energy, thereby reducing the expansion of cracks. The interpenetrating polymer network enhances the toughness of the material, but the flame retardant performance of this modified epoxy resin is poor; Chinese patent document with publication number CN116284511A discloses a method for preparing a strong and tough epoxy resin, an interpenetrating polymer network technology, and a method for preparing a strong and tough epoxy resin. Epoxy resin coating and its application, firstly, 2-(but-3-enyloxy)-3-hydroxypropyl acetate is used as a monomer for addition polymerization to obtain an addition polymer; then the polyunsaturated acid containing a double bond is ring-opened and epoxidized to obtain a long carbon chain epoxide; the addition polymer is grafted onto the long carbon chain epoxide to obtain a strong and tough epoxy resin, and the strong and tough epoxy resin obtained by chemically modifying the original epoxy resin has multiple ester-based flexible chains and linear long carbon chains, which improves the weather resistance and toughness of the epoxy resin, but this strong and tough epoxy resin does not have better high temperature resistance.
[0005] Therefore, it is necessary to provide an epoxy resin having high toughness, high flame retardancy and beautiful cured color for use in the molding of hydrogen storage cylinders. Summary of the invention
[0006] The technical problem solved by the present invention is to provide an epoxy resin composition, a hydrogen storage bottle and a preparation method, with the aim of overcoming the technical disadvantage of poor fire resistance of epoxy resin for hydrogen storage cylinders. By means of toughening modification and flame retardant modification of the target epoxy resin system, an epoxy resin composition having both high toughness and high flame retardancy requirements and suitable for wet winding molding process is prepared. While ensuring the fatigue resistance, high toughness and high fire resistance requirements of the hydrogen storage cylinder, it also has a molding effect with beautiful appearance and no yellowing, thereby meeting the market demand for Type IV gas cylinders.
[0007] In order to solve the above problems, the first aspect of the present invention provides an epoxy resin composition, characterized in that:
[0008] It includes component A and component B;
[0009] The component A comprises the following components in parts by weight: 60 to 90 parts of epoxy resin, 5 to 15 parts of active diluent, 10 to 20 parts of first reactive toughening agent, and 10 to 20 parts of flame retardant;
[0010] The B component includes the following components in parts by mass: 80-100 parts of anhydride curing agent, 0.5-3 parts of accelerator, and 5-10 parts of a second reactive toughening agent;
[0011] The mass ratio of the component A to the component B is 100:92-98.
[0012] Preferably, the A component includes the following components in parts by mass: 74-80 parts of epoxy resin, 5-10 parts of active diluent, 15-16 parts of first reactive toughening agent, and 10-15 parts of flame retardant; the B component includes the following components in parts by mass: 85-95 parts of anhydride curing agent, 1-3 parts of accelerator, and 5-10 parts of second reactive toughening agent.
[0013] Preferably, the viscosity of component A is 100-30000 mPa·s, and the epoxy equivalent is 100-400 g / eq; the viscosity of component B is 10-3000 mPa·s, and the anhydride equivalent is 100-400 g / eq.
[0014] Preferably, the epoxy resin is a mixture of one or more of bisphenol A epoxy resin, bisphenol F epoxy resin and novolac epoxy resin; the active diluent is a mixture of one or more of monofunctional epoxy active diluent, difunctional epoxy active diluent and multifunctional epoxy active diluent.
[0015] Preferably, the first reactive toughening agent is a rubber elastomer, a core-shell toughening agent, or a mixture of one or more of special engineering plastics; the second reactive toughening agent is a polyether mixture, and the polyether is a hydroxyl-terminated polyether, an amine-terminated polyether, a hydroxyl-terminated polyester, or a hydroxyl-terminated polyester ether.
[0016] Preferably, the flame retardant is one or a mixture of dimethyl methylphosphonate, triethyl phosphate, diethyl ethylphosphonate, dimethyl methyl phosphate, triphosphate, tricresyl phosphate, and toluene diphenyl phosphate; the acid anhydride curing agent is one or a mixture of methyltetrahydrophthalic anhydride, tetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, and hexahydrophthalic anhydride; the accelerator is one or a mixture of imidazole accelerators or tertiary amine accelerators.
[0017] A second aspect of the present invention provides a method for preparing the above-mentioned epoxy resin composition, characterized in that it comprises the following steps:
[0018] S1: mixing the epoxy resin, the reactive diluent, the first reactive toughening agent and the flame retardant in proportion by weight to obtain component A;
[0019] S2: mixing the acid anhydride curing agent, the accelerator, and the second reactive toughening agent to obtain component B;
[0020] S3: Mix the component A and the component B to obtain the epoxy resin composition.
[0021] Preferably, in step S2, 1 / 3 of the anhydride curing agent is first mixed with the second reactive toughening agent, and then the remaining 2 / 3 of the anhydride curing agent and the accelerator are added in sequence and mixed to obtain component B.
[0022] Preferably, in step S2, 1 / 3 of the anhydride curing agent and the second reactive toughening agent are first stirred at 65-90°C for 30-40 minutes, and then cooled to 25-35°C; then the remaining 2 / 3 of the anhydride curing agent and the accelerator are added in sequence and mixed, and stirred for 30-40 minutes to obtain component B.
[0023] The third aspect of the present invention provides a hydrogen storage bottle, characterized in that:
[0024] It is made from the above epoxy resin composition.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The epoxy resin composition of the present invention uses a variety of reactive toughening agents to perform synergistic toughening modification on the resin system, so that the product has excellent mechanical properties and heat resistance, wherein Tg≥110°C, tensile strength≥70MPa, tensile modulus≥2800MPa, and elongation at break≥4.5%; by introducing a halogen-free flame retardant into the resin composition, the problems of poor fire resistance of the product, pollution during combustion, and influence on the wettability of the resin and fiber are solved, while ensuring the above-mentioned mechanical and heat resistance, its flame retardant property can reach UL94-V0; it is suitable for a wet winding process, while ensuring the above-mentioned mechanical, heat resistance, and flame retardant properties, the product cured product is translucent, and does not turn yellow after being wound on a gas cylinder and cured. DETAILED DESCRIPTION
[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] The embodiment of the present invention provides an epoxy resin composition:
[0029] It includes component A and component B;
[0030] Component A includes the following components by weight: 60-90 parts of epoxy resin, 5-15 parts of active diluent, 10-20 parts of first reaction type toughening agent, and 10-20 parts of flame retardant;
[0031] Component B includes the following components in parts by weight: 80-100 parts of anhydride curing agent, 0.5-3 parts of accelerator, and 5-10 parts of a second reactive toughening agent;
[0032] The mass ratio of component A to component B is 100:92-98.
[0033] The epoxy resin composition of the present invention uses a variety of reactive toughening agents to perform synergistic toughening modification on the resin system, so that the product has excellent mechanical properties and heat resistance, wherein Tg≥110°C, tensile strength≥70MPa, tensile modulus≥2800MPa, and elongation at break≥4.5%; by introducing a halogen-free flame retardant into the resin composition, the problems of poor fire resistance of the product, pollution during combustion, and influence on the wettability of the resin and fiber are solved, while ensuring the above mechanical properties and heat resistance, its flame retardant property can reach UL94-V0; it is suitable for a wet winding process, while ensuring the above mechanical, heat resistance, and flame retardant properties, the product cured product is translucent, and does not turn yellow after being wound on a gas cylinder and cured.
[0034] Further preferably, the A component includes the following components in mass fractions: 74-80 parts of epoxy resin, 5-10 parts of active diluent, 15-16 parts of first reactive toughening agent, and 10-15 parts of flame retardant; the B component includes the following components in mass fractions: 85-95 parts of anhydride curing agent, 1-3 parts of accelerator, and 5-10 parts of second reactive toughening agent. Within this mass percentage range, the comprehensive performance of epoxy resin coating can be further improved.
[0035] In some embodiments, the viscosity of component A is 100-30000 mPa·s, and the epoxy equivalent is 100-400 g / eq; the viscosity of component B is 10-3000 mPa·s, and the anhydride equivalent is 100-400 g / eq.
[0036] In some embodiments, the epoxy resin is a mixture of one or more of bisphenol A epoxy resin, bisphenol F epoxy resin and novolac epoxy resin; the active diluent is a mixture of one or more of monofunctional epoxy active diluent, difunctional epoxy active diluent and multifunctional epoxy active diluent.
[0037] In some embodiments, the first reactive toughening agent is a rubber elastomer, a core-shell toughening agent, a special engineering plastic, or a mixture of several thereof; the second reactive toughening agent is a polyether mixture, and the polyether is a hydroxyl-terminated polyether, an amine-terminated polyether, a hydroxyl-terminated polyester, or a hydroxyl-terminated polyester ether.
[0038] In some embodiments, the flame retardant is a mixture of one or more of dimethyl methylphosphonate, triethyl phosphate, diethyl ethylphosphonate, dimethyl methyl phosphate, triphosphate, tricresyl phosphate, and toluene diphenyl phosphate; the acid anhydride curing agent is a mixture of one or more of methyltetrahydrophthalic anhydride, tetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, and hexahydrophthalic anhydride; the accelerator is a mixture of one or more of imidazole accelerators or tertiary amine accelerators.
[0039] A second aspect of an embodiment of the present invention provides a method for preparing the above-mentioned epoxy resin composition, comprising the following steps:
[0040] S1: mixing epoxy resin, reactive diluent, first reaction type toughening agent and flame retardant in proportion by weight to obtain component A;
[0041] S2: mixing an anhydride curing agent, an accelerator, and a second reactive toughening agent to obtain component B;
[0042] S3: Mix component A and component B to obtain an epoxy resin composition.
[0043] In some embodiments, in step S2, 1 / 3 of the anhydride curing agent is first mixed with the second reactive toughening agent, and then the remaining 2 / 3 of the anhydride curing agent and the accelerator are sequentially added and mixed to obtain component B.
[0044] The preparation method of the embodiment of the present invention comprises the following steps: mechanically stirring the epoxy resin, the active diluent, the toughening agent and the flame retardant at 50-70° C. at a speed of 400-600 rad / min, mixing for 60-120 minutes, and cooling to room temperature to obtain component A; fully stirring 1 / 3 of the anhydride and the accelerator at 65-90° C. for 30-40 minutes, and cooling to 25-35° C.; sequentially adding the remaining 2 / 3 of the anhydride and the defoaming agent to the mixed solution, fully stirring and mixing for 30-40 minutes to obtain component B; and mixing component A and component B according to the mass ratio to obtain the epoxy resin composition.
[0045] In some embodiments, in step S2, 1 / 3 of the anhydride curing agent and the second reactive toughening agent are firstly mixed at 65 ~ Stir at 90° C. for 30-40 minutes, and cool to 25-35° C.; then add the remaining 2 / 3 of the anhydride curing agent and the accelerator in sequence, mix, and stir for 30-40 minutes to obtain component B.
[0046] A third aspect of an embodiment of the present invention provides a hydrogen storage bottle:
[0047] It is made from the above epoxy resin composition.
[0048] Example 1
[0049] The epoxy resin composition of this embodiment,
[0050] It includes component A and component B;
[0051] Among them, component A includes the following components in parts by mass: 65 parts of E51 liquid epoxy, 10 parts of E-20 solid epoxy, 5 parts of modified polyurethane toughening agent, 10 parts of terminal carboxyl liquid nitrile rubber toughening agent, 10 parts of neopentyl glycol diglycidyl ether, and 10 parts of phosphorus liquid flame retardant;
[0052] Component B includes the following components by weight: 95 parts of methyltetrahydrophthalic anhydride, 10 parts of hydroxyl-terminated polyether, and 1.5 parts of 1-methylimidazole;
[0053] The mass ratio of component A to component B is 100:95.
[0054] The preparation method of the epoxy resin composition of this embodiment comprises the following steps:
[0055] S1: 65 parts of E51 liquid epoxy and 10 parts of E-20 solid epoxy were stirred at 100°C for 40 minutes to fully dissolve and mix; 5 parts of modified polyurethane toughener, 10 parts of terminal carboxyl liquid nitrile rubber toughener, 10 parts of neopentyl glycol diglycidyl ether and 10 parts of phosphorus liquid flame retardant were added at 70°C, and the mixture was stirred and mixed for 20 minutes while maintaining a vacuum degree of not less than -0.07Mpa to obtain component A;
[0056] S2: 30 parts of methyltetrahydrophthalic anhydride and 10 parts of hydroxyl-terminated polyether were stirred at 65°C for 30 minutes, cooled to 35°C, and then 65 parts of methyltetrahydrophthalic anhydride and 1.5 parts of 1-methylimidazole were added in sequence, stirred for 30 minutes, to obtain component B;
[0057] S3: Component A and component B are mixed in a ratio of 100:95 to obtain an epoxy resin composition.
[0058] Example 2
[0059] The epoxy resin composition of this embodiment,
[0060] It includes component A and component B;
[0061] Among them, component A includes the following components in parts by mass: 80 parts of E54 liquid epoxy, 5 parts of carboxyl-terminated liquid nitrile rubber toughening agent, 10 parts of core-shell toughening agent, 5 parts of 1,4-butanediol diglycidyl ether, and 10 parts of phosphorus-based liquid flame retardant;
[0062] Component B includes the following components by weight: 90 parts of methyl hexahydrophthalic anhydride, 10 parts of hydroxyl-terminated polyester ether, and 3 parts of benzyl dimethylamine;
[0063] The mass ratio of component A to component B is 100:92.
[0064] The preparation method of the epoxy resin composition of this embodiment comprises the following steps:
[0065] S1: Add 80 parts of E54 liquid epoxy, 5 parts of carboxyl-terminated liquid nitrile rubber toughener, 10 parts of core-shell toughener, 5 parts of 1,4-butanediol diglycidyl ether, and 10 parts of phosphorus-based liquid flame retardant at 70°C, stir and mix for 40 minutes while maintaining a vacuum degree of not less than -0.07 MPa to obtain component A;
[0066] S2: 30 parts of methyl hexahydrophthalic anhydride and 10 parts of hydroxyl-terminated polyester ether were stirred at 65°C for 30 minutes, and the temperature was lowered to 35°C; 60 parts of methyl hexahydrophthalic anhydride and 3 parts of benzyl dimethylamine were added in sequence, and stirred for 30 minutes to obtain component B;
[0067] S3: Component A and component B are mixed in a ratio of 100:92 to obtain an epoxy resin composition.
[0068] Example 3
[0069] The epoxy resin composition of this embodiment includes component A and component B;
[0070] Among them, component A includes the following components in parts by mass: 72 parts of E54 liquid epoxy, 5 parts of NPEF-170 liquid epoxy, 5 parts of modified polyurethane toughening agent, 10 parts of core-shell toughening agent, 8 parts of 1,6-hexanediol diglycidyl ether, and 15 parts of phosphorus-based liquid flame retardant;
[0071] Component B includes the following components by weight: 90 parts of methyl hexahydrophthalic anhydride, 5 parts of hydroxyl-terminated polyether, and 1 part of 1-methylimidazole;
[0072] The mass ratio of component A to component B is 100:98.
[0073] The preparation method of the epoxy resin composition of this embodiment comprises the following steps:
[0074] S1: Add 72 parts of E54 liquid epoxy, 5 parts of NPEF-170 liquid epoxy, 5 parts of modified polyurethane toughening agent, 10 parts of core-shell toughening agent, 8 parts of 1,6-hexanediol diglycidyl ether, and 15 parts of phosphorus liquid flame retardant at 70°C, stir and mix for 40 minutes while maintaining a vacuum degree of not less than -0.07Mpa, to obtain component A;
[0075] S2: 30 parts of methyl hexahydrophthalic anhydride and 5 parts of hydroxyl-terminated polyether were stirred at 65°C for 30 minutes, and then cooled to 35°C; 60 parts of methyl hexahydrophthalic anhydride and 1 part of 1-methylimidazole were added in sequence, and stirred for 30 minutes to obtain component B;
[0076] S3: Component A and component B are mixed in a ratio of 100:98 to obtain an epoxy resin composition.
[0077] Example 4
[0078] The epoxy resin composition of this embodiment,
[0079] It includes component A and component B;
[0080] Among them, component A includes the following components in parts by mass: 60 parts of E54 liquid epoxy, 14 parts of NPEF-170 liquid epoxy, 8 parts of modified polyurethane toughening agent, 8 parts of core-shell toughening agent, 10 parts of 1,4-butanediol diglycidyl ether, and 15 parts of phosphorus-based liquid flame retardant;
[0081] Component B includes the following components by weight: 90 parts of methyl hexahydrophthalic anhydride, 5 parts of hydroxyl-terminated polyether, and 2 parts of 2-methylimidazole;
[0082] The mass ratio of component A to component B is 100:98.
[0083] The preparation method of the epoxy resin composition of this embodiment comprises the following steps:
[0084] S1: Add 60 parts of E54 liquid epoxy, 14 parts of NPEF-170 liquid epoxy, 8 parts of modified polyurethane toughener, 8 parts of core-shell toughener, 10 parts of 1,4-butanediol diglycidyl ether, and 15 parts of phosphorus liquid flame retardant at 70°C, stir and mix for 40 minutes while maintaining a vacuum degree of not less than -0.07Mpa, to obtain component A;
[0085] S2: 30 parts of methyl hexahydrophthalic anhydride, 5 parts of hydroxyl-terminated polyether, and 2 parts of 2-methylimidazole were stirred at 65°C for 30 minutes, and the temperature was lowered to 35°C; the remaining 60 parts of methyl hexahydrophthalic anhydride were added and stirred for 30 minutes to obtain component B;
[0086] S3: Component A and component B are mixed in a ratio of 100:98 to obtain an epoxy resin composition.
[0087] Example 5
[0088] The epoxy resin composition of this embodiment,
[0089] It includes component A and component B;
[0090] Among them, component A includes the following components in parts by mass: 65 parts of E51 liquid epoxy, 10 parts of E-20 solid epoxy, 5 parts of carboxyl-terminated liquid nitrile rubber toughener, 10 parts of trimethylolpropane triglycidyl ether, and 10 parts of phosphorus-based liquid flame retardant;
[0091] Component B includes the following components by weight: 95 parts of methyltetrahydrophthalic anhydride, 10 parts of hydroxyl-terminated polyether, and 1.5 parts of 1-methylimidazole;
[0092] The mass ratio of component A to component B is 100:95.
[0093] The preparation method of the epoxy resin composition of this embodiment comprises the following steps:
[0094] S1: 65 parts of E51 liquid epoxy and 10 parts of E-20 solid epoxy were stirred at 100°C for 40 minutes to fully dissolve and mix; 5 parts of terminal carboxyl liquid nitrile rubber toughening agent, 10 parts of trimethylolpropane triglycidyl ether and 10 parts of phosphorus liquid flame retardant were added at 70°C, and the mixture was stirred and mixed for 20 minutes while maintaining a vacuum degree of not less than -0.07Mpa to obtain component A;
[0095] S2: 30 parts of methyltetrahydrophthalic anhydride and 10 parts of hydroxyl-terminated polyether were stirred at 65°C for 30 minutes, cooled to 35°C, and then 65 parts of methyltetrahydrophthalic anhydride and 1.5 parts of 1-methylimidazole were added in sequence, stirred for 30 minutes, to obtain component B;
[0096] S3: Component A and component B are mixed in a ratio of 100:95 to obtain an epoxy resin composition.
[0097] Example 6
[0098] The epoxy resin composition of this embodiment,
[0099] It includes component A and component B;
[0100] Among them, component A includes the following components in parts by mass: 80 parts of E54 liquid epoxy, 5 parts of carboxyl-terminated liquid nitrile rubber toughening agent, 10 parts of core-shell toughening agent, 5 parts of trimethylolpropane triglycidyl ether, and 10 parts of phosphorus-based liquid flame retardant;
[0101] Component B includes the following components by weight: 85 parts of methyl hexahydrophthalic anhydride, 5 parts of hydroxyl-terminated polyester ether, and 3 parts of benzyl dimethylamine;
[0102] The mass ratio of component A to component B is 100:92.
[0103] The preparation method of the epoxy resin composition of this embodiment comprises the following steps:
[0104] S1: Add 80 parts of E54 liquid epoxy, 5 parts of carboxyl-terminated liquid nitrile rubber toughener, 10 parts of core-shell toughener, 5 parts of trimethylolpropane triglycidyl ether, and 10 parts of phosphorus liquid flame retardant at 70°C, stir and mix for 40 minutes while maintaining a vacuum degree of not less than -0.07 MPa to obtain component A;
[0105] S2: 25 parts of methyl hexahydrophthalic anhydride and 5 parts of hydroxyl-terminated polyester ether were stirred at 65°C for 30 minutes, and the temperature was lowered to 35°C; the remaining 60 parts of methyl hexahydrophthalic anhydride and 3 parts of benzyl dimethylamine were added in sequence, and stirred for 30 minutes to obtain component B;
[0106] S3: Component A and component B are mixed in a ratio of 100:92 to obtain an epoxy resin composition.
[0107] Example 7
[0108] The epoxy resin composition of this embodiment,
[0109] It includes component A and component B;
[0110] Among them, component A includes the following components in parts by mass: 72 parts of E54 liquid epoxy, 5 parts of NPEF-170 liquid epoxy, 5 parts of modified polyurethane toughening agent, 10 parts of core-shell toughening agent, 8 parts of 1,6-hexanediol diglycidyl ether, and 20 parts of phosphorus-based liquid flame retardant;
[0111] Component B includes the following components by weight: 90 parts of methyl hexahydrophthalic anhydride, 10 parts of hydroxyl-terminated polyether, and 1 part of 1-methylimidazole;
[0112] The mass ratio of component A to component B is 100:98.
[0113] The preparation method of the epoxy resin composition of this embodiment comprises the following steps:
[0114] S1: Add 72 parts of E54 liquid epoxy, 5 parts of NPEF-170 liquid epoxy, 5 parts of modified polyurethane toughening agent, 10 parts of core-shell toughening agent, 8 parts of 1,6-hexanediol diglycidyl ether, and 20 parts of phosphorus liquid flame retardant at 70°C, stir and mix for 40 minutes while maintaining a vacuum degree of not less than -0.07Mpa, to obtain component A;
[0115] S2: 90 parts of methyl hexahydrophthalic anhydride and 10 parts of hydroxyl-terminated polyether were stirred at 65°C for 30 minutes, and then cooled to 35°C; 1 part of 1-methylimidazole was added successively, and stirred for 30 minutes to obtain component B;
[0116] S3: Component A and component B are mixed in a ratio of 100:98 to obtain an epoxy resin composition.
[0117] Example 8
[0118] The epoxy resin composition of this embodiment,
[0119] It includes component A and component B;
[0120] Among them, component A includes the following components in parts by mass: 60 parts of E54 liquid epoxy, 14 parts of NPEF-170 liquid epoxy, 8 parts of modified polyurethane toughening agent, 8 parts of core-shell toughening agent, 10 parts of 1,4-butanediol diglycidyl ether, and 20 parts of phosphorus-based liquid flame retardant;
[0121] Component B includes the following components by weight: 90 parts of methyl hexahydrophthalic anhydride, 5 parts of hydroxyl-terminated polyether, and 2 parts of 2-methylimidazole;
[0122] The mass ratio of component A to component B is 100:95.
[0123] The preparation method of the epoxy resin composition of this embodiment comprises the following steps:
[0124] S1: Add 60 parts of E54 liquid epoxy, 14 parts of NPEF-170 liquid epoxy, 8 parts of modified polyurethane toughening agent, 8 parts of core-shell toughening agent, 10 parts of 1,4-butanediol diglycidyl ether, and 20 parts of phosphorus liquid flame retardant at 70°C, stir and mix for 40 minutes while maintaining a vacuum degree of not less than -0.07Mpa, to obtain component A;
[0125] S2: 30 parts of methyl hexahydrophthalic anhydride, 5 parts of hydroxyl-terminated polyether, and 2 parts of 2-methylimidazole were stirred at 65°C for 30 minutes, and the temperature was lowered to 35°C; the remaining 60 parts of methyl hexahydrophthalic anhydride were added and stirred for 30 minutes to obtain component B;
[0126] S3: Component A and component B are mixed in a ratio of 100:95 to obtain an epoxy resin composition.
[0127] Example 9
[0128] The epoxy resin composition of this embodiment,
[0129] It includes component A and component B;
[0130] Component A includes the following components by weight: 60 parts of E54 liquid epoxy, 5 parts of modified polyurethane toughening agent, 15 parts of neopentyl glycol diglycidyl ether, and 20 parts of phosphorus-based liquid flame retardant;
[0131] Component B includes the following components by weight: 80 parts of methyltetrahydrophthalic anhydride, 20 parts of hydroxyl-terminated polyether, and 3 parts of 1-methylimidazole;
[0132] The mass ratio of component A to component B is 100:92.
[0133] The preparation method of the epoxy resin composition of this embodiment comprises the following steps:
[0134] S1: 60 parts of E54 liquid epoxy were stirred at 100°C for 40 minutes to fully dissolve and mix; 5 parts of modified polyurethane toughening agent, 15 parts of neopentyl glycol diglycidyl ether and 20 parts of phosphorus liquid flame retardant were added at 70°C, and the mixture was stirred and mixed for 20 minutes while maintaining a vacuum degree of not less than -0.07Mpa to obtain component A;
[0135] S2: 30 parts of methyltetrahydrophthalic anhydride and 20 parts of hydroxyl-terminated polyether were stirred at 65°C for 30 minutes, cooled to 35°C, and then 50 parts of methyltetrahydrophthalic anhydride and 3 parts of 1-methylimidazole were added in sequence, stirred for 30 minutes, to obtain component B;
[0136] S3: Component A and component B are mixed in a ratio of 100:92 to obtain an epoxy resin composition.
[0137] Example 10
[0138] The epoxy resin composition of this embodiment,
[0139] It includes component A and component B;
[0140] Component A includes the following components by weight: 80 parts of E54 liquid epoxy, 10 parts of E-20 solid epoxy, 20 parts of modified polyurethane toughening agent, 5 parts of neopentyl glycol diglycidyl ether, and 10 parts of phosphorus-based liquid flame retardant;
[0141] Component B includes the following components in parts by mass: 100 parts of methyltetrahydrophthalic anhydride, 5 parts of hydroxyl-terminated polyether, and 0.5 parts of 1-methylimidazole;
[0142] The mass ratio of component A to component B is 100:98.
[0143] The preparation method of the epoxy resin composition of this embodiment comprises the following steps:
[0144] S1: 80 parts of E54 liquid epoxy and 10 parts of E-20 solid epoxy were stirred at 100°C for 40 minutes to fully dissolve and mix; 20 parts of modified polyurethane toughening agent, 5 parts of neopentyl glycol diglycidyl ether and 5 parts of phosphorus liquid flame retardant were added at 70°C, and the mixture was stirred and mixed for 20 minutes while maintaining a vacuum degree of not less than -0.07Mpa to obtain component A;
[0145] S2: 30 parts of methyltetrahydrophthalic anhydride and 5 parts of hydroxyl-terminated polyether were stirred at 65°C for 30 minutes, cooled to 35°C, and then 70 parts of methyltetrahydrophthalic anhydride and 0.5 parts of 1-methylimidazole were added in sequence, and stirred for 30 minutes to obtain component B;
[0146] S3: Component A and component B are mixed in a ratio of 100:98 to obtain an epoxy resin composition.
[0147] Comparative Example 1
[0148] The epoxy resin composition of this embodiment,
[0149] It includes component A and component B;
[0150] Wherein, component A includes the following components in parts by mass: 90 parts of E51 liquid epoxy and 10 parts of neopentyl glycol diglycidyl ether;
[0151] Component B includes the following components in parts by mass: 90 parts of methyltetrahydrophthalic anhydride and 1 part of 1-methylimidazole;
[0152] The mass ratio of component A to component B is 100:90.
[0153] The preparation method of the epoxy resin composition of this embodiment comprises the following steps:
[0154] S1: 90 parts of E51 liquid epoxy and 10 parts of neopentyl glycol diglycidyl ether were stirred and mixed at 70°C for 40 minutes while maintaining a vacuum degree of not less than -0.07 MPa to obtain component A;
[0155] S2: Mix 90 parts of methyltetrahydrophthalic anhydride and 1 part of 1-methylimidazole, and stir for 30 minutes to obtain component B;
[0156] S3: Component A and component B are mixed in a ratio of 100:90 to obtain an epoxy resin composition.
[0157] Comparative Example 2
[0158] The other components of the epoxy resin composition of this comparative example are the same as those of Example 1, and the preparation method is the same as that of Example 1, except that the first reactive toughening agent is not added.
[0159] Comparative Example 3
[0160] The other components of the epoxy resin composition of this comparative example are the same as those of Example 1, and the other steps of the preparation method are the same as those of Example 1, except that the second reactive toughening agent is not added.
[0161] Comparative Example 4
[0162] The other components of the epoxy resin composition of this comparative example are the same as those of Example 1, and the other steps of the preparation method are the same as those of Example 1, except that the flame retardant is decabromodiphenylethane solid powder flame retardant.
[0163] The curing temperature, mechanical properties and flame retardant properties of the epoxy resin compositions obtained in the above embodiments and comparative examples were tested. The test results are shown in Table 1 below.
[0164] It can be seen from the data in Table 1 that the epoxy resin composition of the present invention can better match the wet winding process, and the resin has good heat resistance, high toughness and excellent flame retardant properties, and is suitable for the molding of hydrogen storage cylinders. It can reduce the safety hazards such as gas explosion caused by combustion during the use of hydrogen storage cylinders. In addition, the appearance of the cylinder is in good condition without obvious yellowing, which is conducive to the market sales of industrial products.
[0165] Table 1 Performance test of epoxy resin compositions of various embodiments and comparative examples
[0166]
[0167]
[0168]
[0169] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. An epoxy resin composition, characterized in that: It includes component A and component B; The component A comprises the following components in parts by weight: 60 to 90 parts of epoxy resin, 5 to 15 parts of active diluent, 10 to 20 parts of first reactive toughening agent, and 10 to 20 parts of flame retardant; The B component includes the following components in parts by mass: 80-100 parts of anhydride curing agent, 0.5-3 parts of accelerator, and 5-10 parts of a second reactive toughening agent; The mass ratio of the component A to the component B is 100:92-98.
2. The epoxy resin composition according to claim 1, characterized in that: The component A comprises the following components in parts by weight: 74-80 parts of epoxy resin, 5-10 parts of active diluent, 15-16 parts of first reactive toughening agent, and 10-15 parts of flame retardant; The B component includes the following components in parts by weight: 85 to 95 parts of an anhydride curing agent, 1 to 3 parts of an accelerator, and 5 to 10 parts of a second reactive toughening agent.
3. The epoxy resin composition according to claim 1, characterized in that: The viscosity of the component A is 100-30000 mPa·s, and the epoxy equivalent is 100-400 g / eq; the viscosity of the component B is 10-3000 mPa·s, and the anhydride equivalent is 100-400 g / eq.
4. The epoxy resin composition according to claim 1, characterized in that: The epoxy resin is one or a mixture of bisphenol A epoxy resin, bisphenol F epoxy resin and novolac epoxy resin; The active diluent is one or a mixture of monofunctional epoxy active diluent, difunctional epoxy active diluent and multifunctional epoxy active diluent.
5. The epoxy resin composition according to claim 1, characterized in that: The first reactive toughening agent is one or a mixture of rubber elastomer, core-shell toughening agent, and special engineering plastics; The second reactive toughening agent is a polyether mixture, and the polyether is a hydroxyl-terminated polyether, an amine-terminated polyether, a hydroxyl-terminated polyester or a hydroxyl-terminated polyester ether.
6. The epoxy resin composition according to claim 1, characterized in that: The flame retardant is one or a mixture of dimethyl methylphosphonate, triethyl phosphate, diethyl ethylphosphonate, dimethyl methyl phosphate, triphosphate, tricresyl phosphate, and diphenyl methyl phosphate; The acid anhydride curing agent is one or a mixture of methyltetrahydrophthalic anhydride, tetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, and hexahydrophthalic anhydride; The accelerator is one or a mixture of imidazole accelerators or tertiary amine accelerators.
7. A method for preparing the epoxy resin composition according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1: mixing the epoxy resin, the reactive diluent, the first reactive toughening agent and the flame retardant in proportion by weight to obtain component A; S2: mixing the acid anhydride curing agent, the accelerator, and the second reactive toughening agent to obtain component B; S3: Mix the component A and the component B to obtain the epoxy resin composition.
8. The method for preparing the epoxy resin composition according to claim 7, characterized in that: In step S2, 1 / 3 of the anhydride curing agent is first mixed with the second reactive toughening agent, and then the remaining 2 / 3 of the anhydride curing agent and the accelerator are added in sequence and mixed to obtain component B.
9. The method for preparing the epoxy resin composition according to claim 8, characterized in that: In step S2, 1 / 3 of the anhydride curing agent and the second reactive toughening agent are first stirred at 65-90°C for 30-40 minutes, and then cooled to 25-35°C; then the remaining 2 / 3 of the anhydride curing agent and the accelerator are added in sequence and mixed, and stirred for 30-40 minutes to obtain component B.
10. A hydrogen storage bottle, characterized in that: The method is made of the epoxy resin composition as described in any one of claims 1 to 6.
Citation Information
Cited By
Flame-retardant fast-curing epoxy resin composition, preparation method thereof and composite material based on epoxy resin composition
CN121006031A