Nano-composite colloid for fresh-keeping coating as well as preparation method and application of nano-composite colloid

By combining nano-zinc oxide with titanium dioxide and coating nano-silicon dioxide, nano-composite colloids to form coating films, the problem of insufficient water absorption and mechanical strength of sodium alginate coating films is solved, significantly improving the antibacterial and fresh-preserving effect of eggs, and prolonging the Shelf life.

CN118879133APending Publication Date: 2024-11-01黄艺畅
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410953770.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing sodium alginate coating films have poor water absorption and low mechanical strength when keeping eggs, resulting in water loss and microbial invasion, limiting its preservation effect.

Method used

Nano zinc oxide is combined with titanium dioxide and coated with nanosilicon dioxide to prepare nanocomposite colloids for preservation to form coating films to enhance antibacterial and gas and moisture barrier capabilities.

Benefits of technology

It significantly improves the antibacterial effect and shelf life of the coating, extends the freshness and shelf life of the eggs, enhances the barrier properties of water vapor and oxygen, and prevents bacterial invasion and water loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879133A_ABST
    Figure CN118879133A_ABST
Patent Text Reader

Abstract

The invention discloses a nano composite colloid for a fresh-keeping coating as well as a preparation method and application of the nano composite colloid. The preparation method comprises the following steps: step 1, preparing a nano zinc oxide colloidal solution; step 2, preparing nano zinc oxide-titanium dioxide mixed sol; step 3, preparing a nano zinc oxide-titanium dioxide composite colloid coated with nano silicon dioxide; step 4, preparing sodium alginate colloid; and step 5, preparing the nano-composite colloid for the fresh-keeping coating film. After the nano-composite colloid obtained by the preparation method disclosed by the invention is prepared into a coating film, the growth of microorganisms on the surfaces of poultry eggs can be effectively inhibited, the invasion of bacteria and oxygen can be prevented, the loss of moisture and CO2 in the eggs can be prevented, and the refreshing time of the poultry eggs can be prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coating preservation, in particular to a nano composite colloid for coating preservation, and a preparation method and application thereof. Background Art

[0002] As one of the most consumed foods in the world, the development of egg preservation technology is crucial. The eggshell has tiny pores that facilitate gas exchange, but also provide a way for microorganisms to invade. Due to the evaporation of water and the action of various internal and external microorganisms, the large amount of nutrients in the eggs will cause irreversible loss of nutrients or even corruption during the storage process, making the eggs susceptible to contamination and deterioration during storage.

[0003] At present, there are many methods for preserving eggs, mainly including refrigeration, controlled atmosphere, irradiation and coating. The coating method has received widespread attention due to its low cost, convenient operation, significant and long-lasting effect. As a natural polysaccharide, sodium alginate has shown significant advantages in the field of egg preservation with its excellent biocompatibility, biodegradability and environmental friendliness. Its excellent film-forming property provides a uniform and stable protective film for eggs, effectively isolating them from external microorganisms and physical damage, while slowing down water loss, maintaining the freshness and nutritional value of eggs, and extending the shelf life of eggs. However, sodium alginate contains more hydroxyl groups, which are easy to form hydrogen bonds with water molecules and have strong water absorption. Therefore, it has poor water vapor barrier properties, and its structure is unstable in a high humidity environment. At the same time, its mechanical strength is low and it is easily damaged during transportation. Therefore, the preservation effect of a simple sodium alginate coating is very limited.

[0004] It should be noted that the information disclosed in the above background technology section is only used for understanding the background of the present application, and therefore may include information that does not constitute prior art known to ordinary technicians in the field. Summary of the invention

[0005] In order to make up for the deficiencies of the prior art, the present invention provides a nano composite colloid for fresh-keeping coating film and a preparation method and application thereof.

[0006] The present invention adopts the following technical solution:

[0007] In a first aspect, a method for preparing a nanocomposite colloid for a fresh-keeping coating is provided, which comprises the following steps:

[0008] Step 1, preparing a nano zinc oxide colloidal solution: preparing a nano zinc oxide colloidal solution at 30-80° C. by a neutralization reaction of zinc acetate and NaOH;

[0009] Step 2, preparing a nano zinc oxide-titanium dioxide mixed sol: at room temperature, slowly drop the tetrabutyl titanate solution into the nano zinc oxide colloidal solution obtained in step 1, and stir at 70° C.-85° C. to obtain a nano zinc oxide-titanium dioxide mixed sol;

[0010] Step 3, preparing nano-silicon dioxide coated nano-zinc oxide-titanium dioxide composite colloid: slowly adding tetraethyl orthosilicate solution to the nano-zinc oxide-titanium dioxide mixed sol obtained in step 2, stirring at 70° C.-80° C. to obtain a mixed colloid; dropping the mixed colloid into a mixed solution containing sodium hexametaphosphate and citric acid, stirring at 70° C.-85° C., and then stirring and aging at room temperature to obtain nano-silicon dioxide coated nano-zinc oxide-titanium dioxide composite colloid;

[0011] Step 4, preparing sodium alginate colloid;

[0012] Step 5, preparing a nano-composite colloid for a fresh-keeping coating: adding the nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite colloid obtained in step 3 accounting for 0.5wt%-2wt% of the sodium alginate colloid obtained in step 4, stirring evenly, and letting it stand to obtain a nano-composite colloid for a fresh-keeping coating.

[0013] In a second aspect, a nanocomposite colloid for fresh-keeping coating prepared by the preparation method described in the first aspect is provided.

[0014] In the third aspect, a nanocomposite colloid for fresh-keeping coating prepared by the preparation method described in the first aspect is provided, wherein the nanocomposite colloid forms a coating directly coated on the outer surface of the object to be preserved or the surface of the food packaging film. The beneficial effects of the present invention include: the present invention significantly improves the antibacterial effect of the coating by compounding nano zinc oxide with titanium dioxide and further coating nano silicon dioxide to obtain a coating, the antibacterial property of nano zinc oxide is combined with the ultraviolet absorption capacity of titanium dioxide to effectively inhibit the growth of microorganisms on the surface of poultry eggs and reduce bacterial invasion and reproduction, and the addition of nano silicon dioxide further enhances the barrier capacity of the coating to gas and moisture, thereby improving the overall fresh-keeping effect of the coating and extending the shelf life of the object to be preserved. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a graph showing the change in weight loss rate of eggs during storage in Experimental Example 1 of the present invention;

[0016] Figure 2 This is a graph showing changes in the Hough unit of eggs during storage in Experimental Example 1 of the present invention;

[0017] Figure 3This is a graph showing changes in the egg yolk index during storage of eggs in Experimental Example 1 of the present invention;

[0018] Figure 4 This is a graph showing the changes in the total bacterial count of eggs during storage in Experimental Example 2 of the present invention. DETAILED DESCRIPTION

[0019] The following is a detailed description of the embodiments of the present invention. It should be emphasized that the following description is only exemplary and is not intended to limit the scope and application of the present invention. In the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other.

[0020] In the present invention, "normal temperature" refers to 20-25°C.

[0021] The specific embodiment of the present invention provides a method for preparing a nanocomposite colloid for a fresh-keeping coating, comprising the following steps:

[0022] Step 1, preparing nano zinc oxide colloidal solution: preparing nano zinc oxide colloidal solution at 30-80° C. through a neutralization reaction of zinc acetate and NaOH.

[0023] In a preferred embodiment, the step 1 comprises: taking 5g-15g of zinc acetate and adding it to 100-200ml of deionized water, stirring evenly, adding dropwise a NaOH solution with a concentration of 4wt%-7wt%, stirring while dropping, and heating it at a temperature of 30-80°C; then transferring the mixed solution to a hydrothermal kettle for heat preservation reaction at a temperature of 30-80°C for a reaction time of 1-6 hours, and obtaining a nano zinc oxide sol after the reaction. Further preferably, the stirring speed is 100r / min-500r / min.

[0024] Step 2, preparing nano zinc oxide-titanium dioxide mixed sol: at room temperature, slowly drop the tetrabutyl titanate solution into the nano zinc oxide colloidal solution obtained in step 1, and stir at 70° C.-85° C. to obtain nano zinc oxide-titanium dioxide mixed sol.

[0025] In a preferred embodiment, the step 2 comprises: dissolving 3 mL to 8 mL of tetrabutyl titanate in 20 mL to 40 mL of anhydrous ethanol at room temperature to obtain a tetrabutyl titanate solution; slowly dropping the tetrabutyl titanate solution (preferably at a rate of 0.5 mL per minute) into 30 mL to 50 mL of the nano zinc oxide sol obtained in step 1, stirring at 70° C. to 85° C. for 45 to 60 minutes to obtain a nano zinc oxide-titanium dioxide mixed sol. Further preferably, the stirring speed is 100 r / min to 500 r / min.

[0026] Step 3, preparing nano-silicon dioxide coated nano-zinc oxide-titanium dioxide composite colloid: slowly dripping tetraethyl orthosilicate solution (preferably at a rate of 0.5 ml per minute) into the nano-zinc oxide-titanium dioxide mixed sol obtained in step 2, stirring at 70°C-80°C to obtain a mixed colloid; dripping the mixed colloid into a mixed solution containing sodium hexametaphosphate and citric acid, stirring at 70°C-85°C, and then stirring and aging at room temperature to obtain nano-silicon dioxide coated nano-zinc oxide-titanium dioxide composite colloid, the average particle size of the composite colloid is <50nm.

[0027] In a preferred embodiment, the step 3 comprises: at room temperature, tetraethyl orthosilicate (TOES) and anhydrous ethanol are mixed in a volume ratio of 1:4 to obtain a tetraethyl orthosilicate solution; the tetraethyl orthosilicate is slowly added to the nano zinc oxide-titanium dioxide mixed sol obtained in step 2, and stirred at 70°C-80°C for 1-2h to obtain a mixed sol; analytically pure sodium hexametaphosphate and citric acid are taken, and mixed in equal volumes to obtain a mixed solution of sodium hexametaphosphate and citric acid; 400μL-500μL of the The mixed solution of sodium hexametaphosphate and citric acid is dissolved in 70mL-100mL of water to obtain the mixed solution containing sodium hexametaphosphate and citric acid; the mixed sol is dripped into the mixed solution containing sodium hexametaphosphate and citric acid according to the volume ratio of the mixed sol to the mixed solution containing sodium hexametaphosphate and citric acid of 1:1-1:1.5, stirred at 70°C-85°C for 4-6h, and then stirred and aged at room temperature for more than 48h to obtain the nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite colloid. Further preferably, the stirring speed is 100r / min-500r / min.

[0028] Step 4, preparing sodium alginate colloid;

[0029] In a preferred embodiment, step 4 comprises: weighing 1g-3g of sodium alginate, adding it to 100ml of deionized water, stirring evenly to obtain a sodium alginate solution, and adding 5-10ml of a 3-4% calcium chloride solution by mass to the sodium alginate solution to obtain a sodium alginate colloid. Further preferably, the stirring speed is 100r / min-500r / min.

[0030] Step 5, preparing a nano-composite colloid for a fresh-keeping coating: adding the nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite colloid obtained in step 3, which accounts for 0.5wt%-2wt% of the sodium alginate colloid, to the sodium alginate colloid obtained in step 4, stirring evenly, and standing to obtain a nano-composite colloid for a fresh-keeping coating. Preferably, the stirring speed is 100r / min-500r / min.

[0031] The above preferred embodiments of the present invention have the following characteristics:

[0032] 1. In step 1, the formation of nano zinc oxide is promoted by the neutralization reaction of zinc acetate and NaOH under heating and hydrothermal conditions, thereby preparing a stable nano zinc oxide colloidal solution. Compared with the prior art, the reaction temperature of this method is relatively low, usually between 30-80°C, with low equipment requirements, and helps to reduce energy consumption and avoid potential risks caused by high temperature.

[0033] 2. Nano zinc oxide has strong antibacterial properties, can effectively inhibit the growth of surface microorganisms such as eggs waiting for preservation, and can absorb ultraviolet rays, provide a certain degree of ultraviolet protection for the preserved objects, slow down the photodegradation process, and under light conditions, nano zinc oxide can produce active substances, which can decompose organic pollutants, have the effects of self-cleaning and disinfection, and are one of the commonly used antibacterial materials at present, but nano zinc oxide is easy to aggregate, affecting its uniform dispersion and performance in the coating, and nano zinc oxide has limited effect on some drug-resistant strains, and the antibacterial coating prepared only with nano zinc oxide has poor antibacterial uniformity, single antibacterial performance, and difficult to ensure the uniformity of the coating, which greatly reduces the antibacterial effect. In step 2, by slowly adding tetrabutyl titanate solution to nano zinc oxide sol and stirring at a certain temperature, uniform mixing of nano zinc oxide and titanium dioxide is achieved. In this process, titanium dioxide is used as a carrier material, and its small size, loose porous structure and large specific surface area help to improve the dispersibility and stability of nano zinc oxide. Through the preparation of this composite material, the antibacterial properties of nano zinc oxide are enhanced, while the light transmittance and biocompatibility of titanium dioxide also provide an additional protective layer for the coating, enhancing the overall performance of the coating. This composite colloid preparation method not only improves the antibacterial uniformity of nano zinc oxide, but also further enhances the antibacterial and fresh-keeping properties of the coating by integrating the characteristics of different materials.

[0034] 3. In step 3, tetraethyl orthosilicate (TOES) is mixed with anhydrous ethanol to prepare tetraethyl orthosilicate solution, and then the tetraethyl orthosilicate solution is slowly added to the nano zinc oxide-titanium dioxide mixed sol prepared in step 2, and stirred at an appropriate temperature to form a nano silicon dioxide coated nano zinc oxide-titanium dioxide composite colloid. In this process, the porous structure and high surface activity of nano silicon dioxide help to improve the dispersibility and stability of nano silicon dioxide coated nano zinc oxide-titanium dioxide composite nanoparticles, while its chemical inertness (with good chemical stability and biocompatibility) provides a stable interface, helps to protect the internal nano zinc oxide and titanium dioxide from the influence of the external environment, and nano silicon dioxide helps to reduce the agglomeration between nanoparticles. In addition, the silicon oxygen bond of nano silicon dioxide can effectively prevent the entry of O2 and other gases and the loss of water, thereby enhancing the barrier performance of the composite coating and further improving the antibacterial and fresh-keeping effect. At the same time, in step 3, the treatment with the mixed solution containing sodium hexametaphosphate and citric acid further promotes the interaction between the nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite nanoparticles, promotes the uniformity of the particle size and the formation of the coating structure, and ensures the stability and uniformity of the nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite colloid. Finally, the obtained nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite colloid has excellent antibacterial properties and preservation effects after being made into a coating.

[0035] 4. In step 4, sodium alginate is used as a base material to prepare a coating. As a natural polysaccharide, sodium alginate has good biocompatibility, biodegradability and environmental friendliness. Its excellent film-forming properties enable sodium alginate to form a uniform and stable protective film, effectively isolating external microorganisms and physical damage, while slowing down water loss and maintaining the freshness and nutritional value of eggs. However, sodium alginate contains more hydroxyl groups, which easily form hydrogen bonds with water molecules and have strong water absorption. Therefore, it has poor water vapor barrier properties, and its structure is unstable in a high humidity environment, and its mechanical strength is low. The sodium alginate used in the specific embodiment of the present invention as a basic material has good biocompatibility, biodegradability and environmental friendliness, and meets the requirements of sustainable development. By using the nano-silicon dioxide treated as above to coat the nano-zinc oxide-titanium dioxide composite colloid to improve the sodium alginate colloid, the mechanical strength and stability of the coating can be significantly improved, the antibacterial properties of the coating can be enhanced, and the barrier properties of the coating to water vapor can be improved, so that the coating can maintain structural stability in a high humidity environment, reducing the degradation of coating performance caused by environmental changes.

[0036] 5. In step 5, the final nano-composite colloid is obtained by adding the nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite colloid to the sodium alginate colloid. After being made into a coating film, it can effectively inhibit the growth of microorganisms on the surface of eggs, prevent the invasion of bacteria and oxygen, prevent the loss of water and CO2 in the eggs, and extend the shelf life of the eggs.

[0037] In summary, the coating made of nano-zinc oxide-titanium dioxide composite colloid coated with nano-silicon dioxide (for example, the coating formed by spraying method) has excellent antibacterial properties and good barrier properties. The antibacterial properties of nano-zinc oxide combined with the ultraviolet absorption ability of titanium dioxide can effectively inhibit the growth of microorganisms on the surface of eggs and provide a certain degree of ultraviolet protection. The addition of nano-silicon dioxide further enhances the barrier ability of the coating to gases (such as O2) and moisture, prevents the loss of moisture and CO2 in the eggs, and thus improves the overall preservation effect of the coating. The final composite sodium alginate colloid can clean and sterilize, prevent the invasion of bacteria and oxygen, prevent the loss of moisture and CO2 in the eggs, keep the pH value of the protein acidic, inhibit the respiration in the eggs, prevent the growth and reproduction of aerobic bacteria, delay the wateriness of egg white, and inhibit the loosening of egg yolk, thereby significantly extending the shelf life of fresh eggs.

[0038] The specific implementation manner of the present invention also includes a nano composite colloid for fresh-keeping coating prepared by the preparation method.

[0039] The specific embodiment of the present invention also includes an application of the nanocomposite colloid for fresh-keeping coating prepared by the preparation method in fresh-keeping, wherein the nanocomposite colloid forms a coating directly covering the outer surface of the object to be preserved or the surface of the food packaging film.

[0040] In a preferred embodiment, the method of directly coating the outer surface of the object to be preserved or the surface of the food packaging film with the nanocomposite colloid is: spraying the nanocomposite colloid on the outer surface of the object to be preserved or the surface of the food packaging film by spraying, air drying or drying, that is, forming a coating on the outer surface of the object to be preserved or the surface of the food packaging film. Preferably, the thickness of the coating is 5μm-20μm.

[0041] In a preferred embodiment, the object to be preserved is poultry eggs or fruit.

[0042] The specific embodiment of the present invention adopts the sol precipitation method to synthesize the nano sol step by step, and then coats it with nano silicon dioxide. The use of a mixed solution containing sodium hexametaphosphate and citric acid in the nano silicon dioxide coating process solves the problems of nano particle agglomeration and uneven dispersion. The specific embodiment of the present invention is further described below. All raw materials in the following embodiments are commercially available.

[0043] Example 1

[0044] The method for preparing the nanocomposite colloid of this embodiment comprises the following steps:

[0045] Step 1: Preparation of nano zinc oxide colloidal solution

[0046] Take 10g of zinc acetate and add it to 100ml of deionized water, stir evenly, add a 4wt% NaOH solution dropwise, stir while adding, and heat it at 60°C; then transfer the mixed solution to a hydrothermal kettle for insulation reaction at 60°C for 2 hours, and obtain nano zinc oxide sol after the reaction.

[0047] Step 2: Preparation of nano zinc oxide-titanium dioxide mixed sol

[0048] At room temperature, 4 mL of tetrabutyl titanate was dissolved in 25 mL of anhydrous ethanol to obtain a tetrabutyl titanate solution.

[0049] The tetrabutyl titanate solution was slowly added dropwise to 30 mL of the nano zinc oxide sol obtained in step 1, and stirred at 70° C. for 45 min to obtain a nano zinc oxide-titanium dioxide mixed sol.

[0050] Step 3: Preparation of nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite colloid

[0051] At room temperature, tetraethyl orthosilicate (TOES) and anhydrous ethanol are mixed in a volume ratio of 1:4 to obtain a tetraethyl orthosilicate solution; the tetraethyl orthosilicate obtained above is slowly added to the nano zinc oxide-titanium dioxide mixed sol in step 2, and stirred at 70° C. for 1 hour to obtain a mixed sol.

[0052] Take analytically pure sodium hexametaphosphate and citric acid, mix them in equal amounts and volumes to obtain a mixed solution of sodium hexametaphosphate and citric acid; take 400 μL of the mixed solution of sodium hexametaphosphate and citric acid, dissolve it in 80 mL of water to obtain an acid catalyst; drop the mixed sol into 80 mL of the acid catalyst, stir at 70° C. for 4 hours, and then stir and age at room temperature for more than 48 hours to obtain a nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite colloid, the average particle size of the composite colloid is <50 nm.

[0053] Step 4: Preparation of sodium alginate colloid

[0054] Weigh 1.5 g of sodium alginate, add it to 100 ml of deionized water, stir evenly to obtain a sodium alginate solution, add 5 ml of a 4% by mass calcium chloride solution to the above solution to obtain a sodium alginate colloid.

[0055] Step 5: Preparation of Nanocomposite Colloids

[0056] The nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite colloid obtained in step 3 is added to the sodium alginate colloid obtained in step 4, accounting for 1 wt % of the above sodium alginate colloid, stirred evenly, and allowed to stand to obtain a nano-composite colloid.

[0057] The nanocomposite colloid prepared above.

[0058] The application of the prepared nanocomposite colloid in the preservation of poultry eggs. The specific method of the poultry egg preservation is: the nanocomposite colloid for poultry egg preservation is sprayed on the shell surface of the poultry egg by a spraying method, and air-dried to form a coating on the outer surface of the poultry egg to preserve the poultry egg and extend its shelf life.

[0059] Example 2

[0060] The method for preparing the nanocomposite colloid of this embodiment comprises the following steps:

[0061] Step 1: Preparation of nano zinc oxide colloidal solution

[0062] Take 10g of zinc acetate and add it to 150ml of deionized water, stir evenly, add 6% NaOH solution drop by drop, stir while adding, and heat it at 70°C. Then transfer the mixed solution to a hydrothermal kettle for heat preservation reaction at 70°C for 1 hour, and obtain nano zinc oxide sol after reaction.

[0063] Step 2: Preparation of nano zinc oxide-titanium dioxide mixed sol

[0064] At room temperature, 3 mL of tetrabutyl titanate was dissolved in 20 mL of anhydrous ethanol to obtain a tetrabutyl titanate solution;

[0065] The tetrabutyl titanate solution was slowly added dropwise to 40 mL of the nano zinc oxide sol obtained in step 1, and stirred at 80° C. for 45 min to obtain a mixed sol.

[0066] Step 3: Preparation of nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite colloid

[0067] At room temperature, tetraethyl orthosilicate (TOES) and anhydrous ethanol are mixed in a volume ratio of 1:4 to obtain a tetraethyl orthosilicate solution; the tetraethyl orthosilicate obtained above is slowly added to the nano zinc oxide-titanium dioxide mixed sol in step 2, and stirred at 80°C for 1.5 hours to obtain a mixed sol. Analytically pure sodium hexametaphosphate and citric acid are taken and mixed in equal amounts and volumes to obtain a mixed solution of sodium hexametaphosphate and citric acid; 500 μL of the mixed solution of sodium hexametaphosphate and citric acid is taken and dissolved in 70 mL of water to obtain an acid catalyst; the mixed sol is dropped into 80 mL of the acid catalyst, stirred at 80°C for 4 hours, and then stirred and aged at room temperature for more than 48 hours to obtain a nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite colloid, the average particle size of the composite colloid is <50 nm.

[0068] Step 4: Preparation of sodium alginate colloid

[0069] Weigh 2 g of sodium alginate, add it to 100 ml of deionized water, stir evenly to obtain a sodium alginate solution, add 8 ml of a 4% by mass calcium chloride solution to the above solution to obtain a sodium alginate colloid.

[0070] Step 5: Preparation of Nanocomposite Colloids

[0071] The nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite colloid obtained in step 3 is added to the sodium alginate colloid obtained in step 4, accounting for 2 wt % of the above sodium alginate colloid, stirred evenly, and allowed to stand to obtain a nano-composite colloid.

[0072] The nanocomposite colloid prepared above.

[0073] The application of the prepared nanocomposite colloid in the preservation of poultry eggs. The specific method of the poultry egg preservation is: the nanocomposite colloid for poultry egg preservation is sprayed on the shell surface of the poultry egg by a spraying method, and air-dried to form a coating on the outer surface of the poultry egg to preserve the poultry egg and extend its shelf life.

[0074] Example 3

[0075] The method for preparing the nanocomposite colloid of this embodiment comprises the following steps:

[0076] Step 1: Preparation of nano zinc oxide colloidal solution

[0077] Take 10g of zinc acetate and add it to 200ml of deionized water, stir evenly, add 7% NaOH solution drop by drop, stir while adding, and heat it at 75°C. Then transfer the mixed solution to a hydrothermal kettle for heat preservation reaction at 75°C for 1.5 hours, and obtain nano zinc oxide sol after reaction.

[0078] Step 2: Preparation of nano zinc oxide-titanium dioxide mixed sol

[0079] At room temperature, 3.5 mL of tetrabutyl titanate was dissolved in 20 mL of anhydrous ethanol to obtain a tetrabutyl titanate solution;

[0080] The tetrabutyl titanate solution was slowly added dropwise to 40 mL of the nano zinc oxide sol obtained in step 1, and stirred at 75° C. for 45 min to obtain a mixed sol.

[0081] Step 3: Preparation of nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite colloid

[0082] At room temperature, tetraethyl orthosilicate (TOES) and anhydrous ethanol are mixed in a volume ratio of 1:4 to obtain a tetraethyl orthosilicate solution; the tetraethyl orthosilicate obtained above is slowly added to the nano zinc oxide-titanium dioxide mixed sol in step 2, and stirred at 75°C for 0.5h to obtain a mixed sol. Analytically pure sodium hexametaphosphate and citric acid are taken and mixed in equal amounts and volumes to obtain a mixed solution of sodium hexametaphosphate and citric acid; 450μL of the mixed solution of sodium hexametaphosphate and citric acid is taken and dissolved in 75mL of water to obtain an acid catalyst; the mixed sol is dropped into 80mL of the acid catalyst, stirred at 75°C for 4h, and then stirred and aged at room temperature for more than 48h to obtain a nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite colloid, the average particle size of the composite colloid is <50nm.

[0083] Step 4: Preparation of sodium alginate colloid

[0084] Weigh 3 g of sodium alginate, add it to 100 ml of deionized water, stir evenly to obtain a sodium alginate solution, add 10 ml of a 4% by mass calcium chloride solution to the above solution to obtain a sodium alginate colloid.

[0085] Step 5: Preparation of Nanocomposite Colloids

[0086] The nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite colloid obtained in step 3 is added to the sodium alginate colloid obtained in step 4, accounting for 1.5 wt % of the above sodium alginate colloid, stirred evenly, and allowed to stand to obtain a nano-composite colloid.

[0087] The nanocomposite colloid prepared above.

[0088] The application of the prepared nanocomposite colloid in the preservation of poultry eggs. The specific method of the poultry egg preservation is: the nanocomposite colloid for poultry egg preservation is sprayed on the shell surface of the poultry egg by a spraying method, and air-dried to form a coating on the outer surface of the poultry egg to preserve the poultry egg and extend its shelf life.

[0089] Experimental Example 1: Egg preservation performance experiment

[0090] The experiment set up a sodium alginate colloid coating test group 2 (test group 2, as a control), the nano-composite colloid coating test group 1 for fresh-keeping coating of the present invention, and a blank test group (blank group, as a control). Specifically, take fresh egg shells, and use a spray method to spray the sodium alginate colloid prepared in step 4 of Example 1 of the present invention as test group 1, the nano-composite colloid of Example 1 of the present invention as test group 2, and no solution is sprayed as a blank control. During the egg preservation period, the freshness of the eggs is evaluated by measuring the changes in weight loss rate, Haugh unit, and yolk index. Details are as follows:

[0091] (1) Changes in weight loss rate

[0092] After the eggs are coated and stored at room temperature, the weight loss rate changes are shown in Figure 1 . Figure 1 It shows that as the storage time increases, the eggs respire and the water inside the eggs is released through the pores on the eggshell surface, and gas exchange is carried out inside and outside, and the weight loss rate continues to increase. The weight loss rate of eggs during storage is: uncoated (blank group) > sodium alginate colloid coating (experimental group 2) > nanocomposite colloid coating (experimental group 1). It can be seen that the weight loss rate of eggs in experimental group 1 is significantly lower than that of eggs in experimental group 2 and the blank group.

[0093] (2) Changes in Hough Units

[0094] After the eggs were coated and stored at room temperature, the changes in their Haugh units were as follows: Figure 2 The Haugh unit is closely related to the quality of eggs. Generally, the Haugh unit of fresh eggs is above 72, and such eggs are called "AA" grade. Figure 2 It can be seen that as the storage time increases, the Haugh unit of eggs shows a downward trend. The results show that the Haugh unit of eggs in test group 1 has a significantly lower downward trend than that of eggs in test group 2 and the blank group.

[0095] (3) Changes in yolk index

[0096] After the eggs are coated and stored at room temperature, the changes in the yolk index are shown in Figure 3 As the storage time increases, the yolk gradually changes from a nearly spherical shape to a flat shape. The fresher the egg, the taller the yolk and the smaller the diameter, and the greater the yolk index. The size of the yolk index of an egg can well reflect the freshness of the egg. Analysis Figure 3 It can be seen that the yolk index of the eggs in test group 1 is significantly higher than that of the eggs in test group 2 and the blank group.

[0097] Experimental Example 2: Experiment on Sterilization Effect

[0098] The experiment set up sodium alginate colloid coating test group 2 (test group 2, as a control), the nanocomposite colloid coating test group 1 for fresh-keeping coating of the present invention, and a blank test group (blank group, as a control). Specifically, take a fresh egg shell and treat the egg surface by spraying (the treatment process is the same as in Experimental Example 1). During storage, the total number of colonies inside the egg is detected and the results are calculated according to GB4789.2-2022 "National Food Safety Standard Food Microbiology Test Colony Count Determination".

[0099] During storage, as the freshness of eggs decreases, the total number of colonies in the egg contents will also change accordingly. The change pattern is shown in Figure 4 (Total number of colonies / (10 5 CFU / 100g)). Figure 4 The results show that in the early stage of storage (such as within the 7th day), the total number of colonies inside the eggs is very small, almost non-existent; as the storage time increases, the total number of colonies inside the eggs will slowly increase; in the late stage of storage (such as from the 14th day onwards), the total number of colonies inside the eggs will increase rapidly. Figure 4 It can also be seen that the microorganisms in test group 2 are lower than those in the blank group and test group 1, indicating that the nanocomposite colloid coating can effectively inhibit the growth of microorganisms. It can also explain that microorganisms are the main reason for the spoilage of eggs.

[0100] The above is an example of eggs. Experiments have shown that the nanocomposite colloid obtained by the preparation method of the present invention can be cleaned and sterilized after forming a coating, prevent the invasion of bacteria and oxygen, prevent the loss of water and CO2 in the egg, keep the protein pH acidic, inhibit the respiration in the egg, prevent the growth and reproduction of aerobic bacteria, delay the wateriness of egg white, inhibit the loosening of yolk, and extend the shelf life of fresh eggs. The pure sodium alginate colloid coating generally has a shelf life of 14-28 days for eggs, while the nanocomposite colloid coating in the present invention has a shelf life of 45 days for eggs, which is 17-31 days longer than the pure sodium alginate coating.

[0101] The nano composite colloid preparation method of the present invention is simple to operate, low in cost, easy to promote and apply, suitable for large-scale production, and provides a new efficient and economical technology for preserving fresh-keeping objects such as poultry eggs.

[0102] In addition to being used for preserving poultry eggs, the nanocomposite colloid of the present invention can also be used for preserving fruits and for food packaging.

[0103] The above content is a further detailed description of the present invention in combination with specific / preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, without departing from the concept of the present invention, it can also make several substitutions or modifications to these described embodiments, and these substitutions or modifications should be regarded as belonging to the protection scope of the present invention. In the description of this specification, the description of the reference terms "an embodiment", "some embodiments", "preferred embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in combination with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily target the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In the absence of mutual contradiction, those skilled in the art can combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples. Although the embodiments of the present invention and their advantages have been described in detail, it should be understood that various changes, substitutions and modifications can be made herein without departing from the scope of protection of the patent application.

Claims

1. A method for preparing a nanocomposite colloid for fresh-keeping coating, characterized in that: The steps include: Step 1, preparing a nano zinc oxide colloidal solution: preparing a nano zinc oxide colloidal solution at 30-80° C. by a neutralization reaction of zinc acetate and NaOH; Step 2, preparing a nano zinc oxide-titanium dioxide mixed sol: at room temperature, slowly drop the tetrabutyl titanate solution into the nano zinc oxide colloidal solution obtained in step 1, and stir at 70° C.-85° C. to obtain a nano zinc oxide-titanium dioxide mixed sol; Step 3, preparing nano-silicon dioxide coated nano-zinc oxide-titanium dioxide composite colloid: slowly adding tetraethyl orthosilicate solution to the nano-zinc oxide-titanium dioxide mixed sol obtained in step 2, stirring at 70° C.-80° C. to obtain a mixed colloid; dropping the mixed colloid into a mixed solution containing sodium hexametaphosphate and citric acid, stirring at 70° C.-85° C., and then stirring and aging at room temperature to obtain nano-silicon dioxide coated nano-zinc oxide-titanium dioxide composite colloid; Step 4, preparing sodium alginate colloid; Step 5, preparing a nano-composite colloid for a fresh-keeping coating: adding the nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite colloid obtained in step 3 accounting for 0.5wt%-2wt% of the sodium alginate colloid obtained in step 4, stirring evenly, and letting it stand to obtain a nano-composite colloid for a fresh-keeping coating.

2. The preparation method according to claim 1, characterized in that The step 1 comprises: 5g-15g of zinc acetate is added to 100-200ml of deionized water, stirred evenly, and a NaOH solution with a concentration of 4wt%-7wt% is added dropwise while stirring, and heated at 30-80°C; then the mixed solution is transferred to a hydrothermal kettle for heat preservation reaction at 30-80°C for 1-6 hours, and nano zinc oxide sol is obtained after the reaction.

3. The preparation method according to claim 1, characterized in that: The step 2 comprises: dissolving 3 mL to 8 mL of tetrabutyl titanate in 20 mL to 40 mL of anhydrous ethanol at room temperature to obtain a tetrabutyl titanate solution; The tetrabutyl titanate solution is slowly added dropwise to 30 mL to 50 mL of the nano zinc oxide sol obtained in step 1, and stirred at 70° C. to 85° C. for 45 to 60 min to obtain a nano zinc oxide-titanium dioxide mixed sol.

4. The preparation method according to claim 1, characterized in that: The step 3 comprises: At room temperature, tetraethyl orthosilicate (TOES) and anhydrous ethanol are mixed in a volume ratio of 1:4 to obtain a tetraethyl orthosilicate solution; the tetraethyl orthosilicate is slowly added to the nano zinc oxide-titanium dioxide mixed sol obtained in step 2, and stirred at 70° C.-80° C. for 1-2 hours to obtain a mixed sol; Take analytically pure sodium hexametaphosphate and citric acid, mix them in equal volumes, and obtain a mixed solution of sodium hexametaphosphate and citric acid; take 400 μL-500 μL of the mixed solution of sodium hexametaphosphate and citric acid, dissolve it in 70 mL-100 mL of water, and obtain the mixed solution containing sodium hexametaphosphate and citric acid; according to the volume ratio of the mixed sol to the mixed solution containing sodium hexametaphosphate and citric acid being 1:1-1:1.5, drop the mixed sol into the mixed solution containing sodium hexametaphosphate and citric acid, stir at 70°C-85°C for 4-6 hours, and then stir and age at room temperature for more than 48 hours to obtain a nano-silicon dioxide-coated nano-zinc oxide-titanium dioxide composite colloid.

5. The preparation method according to claim 1, characterized in that: The step 4 comprises: Weigh 1g-3g of sodium alginate, add it into 100ml of deionized water, stir evenly to obtain a sodium alginate solution, add 5-10ml of a calcium chloride solution with a mass fraction of 3-4% into the sodium alginate solution to obtain a sodium alginate colloid.

6. The preparation method according to any one of claims 2 to 5, characterized in that: The stirring speed in any one of steps 1-5 is 100 r / min-500 r / min.

7. A nanocomposite colloid for fresh-keeping coating prepared by the preparation method according to any one of claims 1 to 6.

8. Use of a nanocomposite colloid for fresh-keeping coating prepared by the preparation method according to any one of claims 1 to 6 in fresh-keeping, characterized in that: The nano composite colloid forms a coating film which is directly coated on the outer surface of the object to be preserved or the surface of the food packaging film.

9. The use according to claim 8, characterized in that The method of directly covering the outer surface of the object to be preserved or the surface of the food packaging film with the nano-composite colloid to form a coating is as follows: the nano-composite colloid is sprayed on the outer surface of the object to be preserved or the surface of the food packaging film by a spraying method, and air-dried or baked to form a coating on the outer surface of the object to be preserved or the surface of the food packaging film.

10. The use according to claim 8 or 9, characterized in that: The coating film has a thickness of 5 μm-20 μm; the objects to be preserved are poultry eggs or fruits.

Citation Information

Patent Citations

  • Preparation method for sodium alginate-nano silicon dioxide compound film

    CN104788706A

  • Preparation method of water-based zinc-titanium composite slurry

    CN105542512A

  • Method for preparing zinc oxide nano-colloid solution

    CN109721094A