Preparation method of aluminum strip self-repairing conductive coating for submarine cable armoring
Through microfluidic control technology, beaded structural fibers and conductive coatings are prepared, combined with conductive fillers and modifiers, the problems of low repair efficiency and poor conductivity of the conductive coating of submarine cable armored aluminum alloy in the submarine environment are solved, and high Conductive aluminum tape conductive coating with conductivity and self-healing capabilities extends cable life and reduces safety risks.
Patent Information
- Application Number
- CN202410956929.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-01
AI Technical Summary
The existing aluminum alloy conductive coating for submarine cable armor is problem of low repair efficiency and poor conductivity in complex submarine environments.
Microfluidic control technology is used to prepare beaded structural fibers, and combined with conductive polymers, conductive fillers, curing agents and modifiers, through multi-dentate chelation and thermal curing, aluminium tape conductivity with high conductivity and self-healing ability is formed. coating.
It improves the overall conductivity and self-repair capability of the aluminum tape conductive coating, extends the service life of the cable, and reduces maintenance and safety risks.
Smart Images

Figure CN118879154A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of cable conductive materials, and in particular relates to a method for preparing an aluminum tape self-repairing conductive coating for submarine cable armor. Background Art
[0003] The armor layer of submarine cables refers to a layer of protective material wrapped around the outer layer of the cable, which is used to enhance the mechanical strength and damage resistance of the cable, effectively prevent physical damage and corrosion of seabed salt water in complex seabed environments, extend the service life of the cable, and ensure the safe operation of the cable. At the same time, submarine cables transmit high voltage currents, and the armor of the outer layer of the cable can provide additional electrical shielding. Aluminum alloy replaces stainless steel as the armor material of submarine cables, which has many advantages such as light weight, good corrosion resistance, high cost-effectiveness, excellent thermal conductivity and good environmental performance. However, the performance of aluminum alloy itself is difficult to use as an armor layer for a long time in complex seabed conditions, so the armored aluminum strip needs to be modified for corrosion resistance. However, in the process of manufacturing and erecting cables, due to the influence of the preparation process and aging due to long-term operation, the conductive protective layer of aluminum alloy will inevitably cause micro-crack damage during the erection process. The introduction of self-healing materials can well solve the micro-damage on the surface of the cable protective layer. When micro-cracks occur in the cable armor material, it can actively repair and restore its function, avoiding the problem of difficulty in maintenance and replacement, and has important research value in the field of manufacturing and maintenance of cable conductive protective materials. However, the self-repairing cable conductive protective materials prepared by the prior art have the problems of low repair efficiency or poor conductive performance.
[0004] Patent name: Polymerizable low eutectic solvent for self-healing materials, conductive elastomer and preparation method, announcement number: CN111253520B The invention patent discloses a polymerizable low eutectic solvent for self-healing materials, a conductive elastomer and a preparation method thereof. First, a polymerizable low eutectic solvent, a cross-linking agent and an initiator are used to prepare a matrix without adding conductive nanomaterials. The obtained self-healing conductive elastomer has a transparent appearance, excellent self-healing performance and good environmental stability. However, the overall conductive performance is poor, the selection and ratio of raw materials are very strict, and it is difficult to obtain a self-healing function.
[0005] Patent name: Self-repairing nano-conductive polymer material and preparation method thereof, announcement number: CN105111689B, the invention patent discloses a self-repairing nano-conductive polymer material and preparation method thereof, firstly, a thiol-based liquid polysulfide rubber is added dropwise to bisphenol A epoxy resin to prepare a matrix, and then conductive nanoparticles, curing agent and catalyst are mixed evenly at room temperature. The material has both self-repairing and conductivity. However, the conductive particles are firmly embedded, which reduces the repair effect.
[0006] Patent name: A self-repairing conductive adhesive and its preparation method, announcement number: CN103666318B The invention patent discloses a method for preparing a self-repairing conductive adhesive. First, epoxy resin-porous carbon material powder is used to prepare microcapsule powder, and then the microcapsule powder, epoxy resin, and flaky silver powder are mixed evenly at room temperature. The porous carbon powder wrapped in microcapsules is mainly used to repair cracks and increase conductivity. However, there is a problem that too much microcapsule resin is added, which affects the conductivity of the material.
[0007] Patent name: A high-temperature self-repairing conductive silver paste and its preparation method, announcement number: CN103194164B, the invention patent discloses a method for preparing a high-temperature self-repairing conductive silver paste, using epoxy resin-nano silver wire to prepare microcapsules, mainly using nano silver wire and liquid epoxy resin to release and fill cracks, achieving dual repair of cracks and conductive networks. However, there are more diluents and curing agents in the microcapsules, and volatilization will cause volume shrinkage, affecting the strength of the cracks after repair, affecting the repair rate, and polluting the environment. Summary of the invention
[0008] The purpose of the present invention is to solve the problems of low repair efficiency and poor conductivity of the conductive coating in the above-mentioned prior art, and to provide a method for preparing a self-repairing conductive coating of aluminum strip for submarine cable armor that can overcome the above-mentioned technical problems.
[0009] A method for preparing a self-repairing conductive coating of an aluminum tape for submarine cable armoring of the present invention comprises the following steps: Step 1: Prepare beaded fiber The pH response solution is dissolved in N, N-dimethylformamide to obtain a shell material, and the conductive polymer is dissolved in N, N-dimethylformamide to obtain a core material. The flow rates of the microfluidic dripping system of the shell material and the core material are adjusted respectively by microfluidic technology, so that the shell material is wrapped around the outside of the core material to obtain a beaded structure fiber; Step 2: Formulate the conductive self-healing coating Add the beaded structure fiber obtained in step 1 to the conductive polymer, and add a conductive filler, a curing agent, a modifier, and a defoaming agent at the same time, heat and stir to obtain a conductive self-healing coating; Step 3: Multi-tooth chelating treatment on the surface of aluminum strip The aluminum strip is cleaned in ethanol, corroded in an acid solution, rinsed with deionized water, and subjected to a multi-dentate chelating reaction in a multi-dentate chelating agent citric acid aqueous solution to obtain an aluminum strip with a multi-dentate chelating surface. Step 4: Preparation of conductive self-healing coating The aluminum strip after the multi-tooth chelating treatment obtained in step 3 is immersed in the heated conductive self-healing coating to obtain an impregnated aluminum strip; Step 5: Dust removal and curing reaction The impregnated aluminum strip obtained in step 4 is placed in a dust removal chamber for heat curing treatment, and then the aluminum strip obtained by deionization washing and drying has a self-repairing conductive coating.
[0010] Preferably, the pH response solution in step 1 is any one of poly(silver acrylate) and poly(lactic acid); Preferably, the conductive polymer solution in step 1 is any one of sulfonated polyaniline and poly (3,4-ethylenedioxythiophene); Preferably, the mass ratio of the pH responsive material to N,N-dimethylformamide in the shell layer is (50-80):100, and the mass ratio of the conductive polymer solution to N,N-dimethylformamide in the core layer is (25-50):100; Preferably, the infusion system uses a propulsion pump, the propulsion speed of the core material propulsion pump is (0.05~1) mL / h, and the propulsion speed of the shell material propulsion pump is (0.1~2) mL / h; Preferably, the conductive self-healing coating in step 2 is composed of the following substances by mass percentage: 5% to 10% beaded structure fiber, 69% to 78% conductive polymer, 6% to 13% conductive filler, 4% to 8% curing agent, 1% to 2% modifier, and 1% to 3% defoaming agent; Preferably, the conductive polymer in step 2 is any one of diethylenetriamine and modified polyethylene emulsion; the conductive filler is any one of graphene, carbon black and carbon nanotubes; the curing agent is any one of soybean oil epoxy resin and epoxy resin; the modifier is histamine; and the defoaming agent is aminopropylmethyldiethoxysilane; Preferably, the heating temperature in step 2 is 35°C to 50°C, the stirring rate is 500 rpm, and the time is 0.5h to 1h; Preferably, the cleaning in step 3 is soaking in ethanol for 2 min to 5 min, soaking in an acid solution with a pH of 4 to 5 for 1 min to 3 min, and soaking in a citric acid aqueous solution for 15 min to 30 min, wherein the mass percentage of citric acid is 5% to 10%; Preferably, the acid solution in step 3 has a pH of 4 to 5 and is any one of a sulfuric acid solution and a nitric acid solution; Preferably, the immersion treatment temperature in step 4 is 35°C to 50°C, and the treatment time is 5min to 10min; Preferably, in step 5, the heat curing time is 30 min to 60 min, the temperature of the deionized water is 50° C. to 60° C., the rinsing time is 6 min to 9 min, and the drying temperature is 60° C. to 70° C.
[0011] The present invention adopts microfluidic technology, adjusts the concentration of the core layer solution and wraps it with a pH response solution to obtain a beaded structure fiber with ion switch conductive performance, so that the armored aluminum strip coating has a self-repairing effect; conductive fillers, curing agents, and defoaming agents are added to the conductive polymer for mixing and stirring, and the conductive agent is closely combined with the conductive filler, and the cross-linking effect of the polymer is fully utilized to adjust the proportion of the conductive filler, effectively improve the overall conductive performance of the coating, and at the same time, a modified curing agent is used to reduce the impact on the overall conductivity of the material; the aluminum strip is subjected to alcohol washing and acid washing treatment on the surface, and then reacted with a multi-tooth chelating agent citric acid aqueous solution to obtain an aluminum strip with a multi-tooth chelating treatment on the surface; and the aluminum strip is subjected to dipping and curing treatment in sequence to obtain an aluminum strip with high conductivity and a self-repairing conductive coating. The beneficial effects of the present invention are as follows: beaded structure fibers are constructed by microfluidic technology, and when the armored aluminum strip prepared by the present invention is impacted by external force or the surface of the cable is damaged, local microcracks or seawater infiltration occurs, the fiber shell actively releases the internal conductive polymer, effectively repairs the defects, improves the service life of the cable, and reduces the safety risks during use; the conductive agent and the conductive filler are closely combined, the cross-linking effect of the polymer is fully utilized, the proportion of the conductive filler is adjusted, and the overall conductive performance of the coating is effectively improved; at the same time, a modified curing agent is used to reduce the impact on the overall conductivity of the coating; the surface of the aluminum strip is cleaned multiple times and aluminum chelating agent citric acid is added to improve the bonding strength with the coating, and the overall conductive performance of the coating is effectively improved. The present invention has broad application prospects in the field of conductive coatings. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 It is a schematic diagram of the morphology of the aluminum tape self-repairing conductive coating for submarine cable armoring of the present invention. DETAILED DESCRIPTION
[0013] The present invention is described in detail below with reference to the accompanying drawings.
[0014] Example 1 A method for preparing a self-repairing conductive coating of an aluminum tape for submarine cable armoring in this embodiment comprises the following steps: Step 1: Dissolve 50 g of silver polyacrylate in 100 ml of N,N-dimethylformamide, and pass it through the shell layer propulsion pump at a propulsion speed of 0.1 mL / h. Dissolve 25 g of sulfonated polyaniline in 100 ml of N,N-dimethylformamide, and pass it through the core layer propulsion pump at a propulsion speed of 0.05 mL / h to obtain beaded structure fibers.
[0015] Step 2: Add 5 g of beaded structure fiber, 13 g of self-conductive graphene, 4 g of histamine-modified soybean oil epoxy resin, and 3 g of aminopropylmethyldiethoxysilane to 69 g of diethylenetriamine, heat to 50° C., at a rate of 500 rpm, and stir for 1 hour to obtain an impregnation solution.
[0016] Step 3: The aluminum strip was washed in ethanol for 5 minutes, then corroded in a nitric acid solution with a pH of 4 for 3 minutes, washed with deionized water, and reacted in a 5% citric acid solution for 30 minutes to obtain a surface-chelated aluminum strip.
[0017] Step 4: Place the aluminum strip obtained in step 3 in an impregnation solution heated to 40° C. and soak for 10 minutes to obtain an impregnated aluminum strip.
[0018] Step 5: Place the impregnated aluminum strip obtained in step 4 in a dust removal chamber and allow it to stand, heat it to 70° C. and cure it for 60 minutes. The obtained aluminum strip has a self-healing conductive coating.
[0019] Example 2 A method for preparing a self-repairing conductive coating of an aluminum tape for submarine cable armoring in this embodiment comprises the following steps: Step 1: Dissolve 50 g of polylactic acid in 100 ml of N,N-dimethylformamide, and pass it through the shell layer propulsion pump at a propulsion speed of 1 mL / h. Dissolve 35 g of sulfonated polyaniline in 100 ml of N,N-dimethylformamide, and pass it through the core layer propulsion pump at a propulsion speed of 0.5 mL / h to obtain beaded structure fibers.
[0020] Step 2: Add 10 g of fiber, 6 g of carbon nanotubes, 5 g of organic amine-modified epoxy resin, and 1 g of aminopropylmethyldiethoxysilane to 78 g of modified polyethylene emulsion, heat to 50° C., at a speed of 500 rpm, and stir for 1 hour to obtain an impregnation solution.
[0021] Step 3: The aluminum strip was washed in ethanol for 2 minutes, then corroded in a sulfuric acid solution with a pH of 4 for 1 minute, washed with deionized water, and reacted in a 10% citric acid solution for 15 minutes to obtain a surface-chelated aluminum strip.
[0022] Step 4: Place the aluminum strip obtained in step 3 in an impregnation solution heated to 50° C. and soak for 5 minutes to obtain an impregnated aluminum strip.
[0023] Step 5: Place the impregnated aluminum strip obtained in step 4 in a dust removal chamber and allow it to stand, heat it to 60° C. and cure it for 30 minutes. The obtained aluminum strip has a self-healing conductive coating.
[0024] Example 3 A method for preparing a self-repairing conductive coating of an aluminum tape for submarine cable armoring in this embodiment comprises the following steps: Step 1: Dissolve 80 g of silver polyacrylate in 100 ml of N,N-dimethylformamide, and pass it through a shell layer propulsion pump at a propulsion speed of 2 mL / h. Dissolve 45 g of poly (3,4-ethylenedioxythiophene) in 100 ml of N,N-dimethylformamide, and pass it through a core layer propulsion pump at a propulsion speed of 1 mL / h to obtain a beaded structure fiber.
[0025] Step 2: Add 10 g of fiber, 6 g of conductive carbon black, 5 g of organic amine-modified epoxy resin, and 1 g of aminopropylmethyldiethoxysilane to 78 g of diethylenetriamine, heat to 35°C, stir at a speed of 500 rpm for 0.5 h, and obtain an impregnation solution.
[0026] Step 3: The aluminum strip was washed in ethanol for 2 minutes, then corroded in a sulfuric acid solution with a pH of 5 for 1 minute, washed with deionized water, and then immersed in an 8% citric acid solution for 20 minutes to obtain a surface-chelated aluminum strip.
[0027] Step 4: Place the aluminum strip obtained in step 3 in an impregnation solution heated to 35° C. and soak for 10 minutes to obtain an impregnated aluminum strip.
[0028] Step 5: Place the impregnated aluminum strip obtained in step 4 in a dust removal chamber and allow it to stand, heat it to 70° C. and cure it for 30 minutes. The obtained aluminum strip has a self-healing conductive coating.
[0029] Example 4 A method for preparing a self-repairing conductive coating of an aluminum tape for submarine cable armoring in this embodiment comprises the following steps: Step 1: Dissolve 80 g of polylactic acid in 100 ml of N,N-dimethylformamide, and pass it through the shell layer propulsion pump at a propulsion speed of 1.5 mL / h. Dissolve 50 g of poly (3,4-ethylenedioxythiophene) in 100 ml of N,N-dimethylformamide, and pass it through the core layer propulsion pump at a propulsion speed of 1 mL / h to obtain beaded structure fibers.
[0030] Step 2: Add 5 g of fiber, 13 g of carbon nanotubes, 8 g of histamine-modified soybean oil epoxy resin, and 3 g of aminopropylmethyldiethoxysilane into 74 g of modified polyethylene emulsion, heat to 50° C., at a speed of 500 rpm, and stir for 0.5 h to obtain an impregnation solution.
[0031] Step 3: The aluminum strip was washed in ethanol for 5 minutes, then immersed in a nitric acid solution with a pH of 5 for 3 minutes, washed with deionized water, and then immersed in a 15% citric acid solution for 30 minutes to obtain a surface-chelated aluminum strip.
[0032] Step 4: The aluminum strip obtained in step 3 is placed in an impregnation solution heated to 35° C., and an impregnated aluminum strip is obtained by immersion treatment for 10 minutes.
[0033] Step 5: Place the impregnated aluminum strip obtained in step 4 in a dust removal chamber and allow it to stand, heat it to 60° C. and cure it for 60 minutes. The obtained aluminum strip has a self-healing conductive coating.
[0034] Table 1 Self-repair rate, self-repair time and resistivity of coatings in the examples and conventional self-repair coatings
[0035] Attached Figure 1 The schematic diagram of the self-repairing conductive coating of aluminum strip prepared by the present invention is shown in FIG. Figure 1 It can be seen that the self-repairing beaded structure fiber 1 and the conductive filler 3 are evenly distributed inside the conductive self-repairing coating 2. The conductive filler 3 forms a continuous conductive network, and cooperates with the conductive polymer in the matrix of the conductive self-repairing coating 2 to play a conductive role, so that the coating has excellent conductive properties. The self-repairing beaded structure fiber 1 can release the conductive polymer 4 to repair the conductive self-repairing coating after the coating is damaged by the outside world.
Claims
1. A method for preparing a self-repairing conductive coating of aluminum tape for submarine cable armor, characterized in that The following steps are involved: Step 1: Prepare beaded fiber The pH response solution is dissolved in N,N-dimethylformamide to obtain a shell material, and the conductive polymer solution is dissolved in N,N-dimethylformamide to obtain a core material. The flow rates of the microfluidic dripping system of the shell material and the core material are adjusted respectively by microfluidic technology, so that the shell material is wrapped around the outside of the core material to obtain a beaded structure fiber; Step 2: Formulate the conductive self-healing coating Add the beaded structure fiber obtained in step 1 to the conductive polymer, and add a conductive filler, a curing agent, a modifier, and a defoaming agent at the same time, heat and stir to obtain a conductive self-healing coating; Step 3: Multi-tooth chelating treatment on the surface of aluminum strip The aluminum strip is cleaned in ethanol, corroded in an acid solution, rinsed with deionized water, and subjected to a multi-dentate chelating reaction in a multi-dentate chelating agent citric acid aqueous solution to obtain an aluminum strip with a multi-dentate chelating surface. Step 4: Preparation of conductive self-healing coating The aluminum strip after the multi-tooth chelating treatment obtained in step 3 is immersed in the heated conductive self-healing coating to obtain an impregnated aluminum strip; Step 5: Dust removal and curing reaction The impregnated aluminum strip obtained in step 4 is placed in a dust removal chamber for heat curing treatment, and then the aluminum strip obtained by deionization washing and drying has a self-repairing conductive coating.
2. A method for preparing a self-repairing conductive coating of aluminum tape for submarine cable armor according to claim 1, characterized in that The pH response solution in step 1 is any one of poly(silver acrylate) and poly(lactic acid); The conductive polymer solution in step 1 is any one of sulfonated polyaniline and poly (3,4-ethylenedioxythiophene).
3. A method for preparing a self-repairing conductive coating of aluminum tape for submarine cable armor according to claim 1 or 2, characterized in that The mass ratio of the pH responsive material to N,N-dimethylformamide in the shell layer is (50-80):100, and the mass ratio of the conductive polymer solution to N,N-dimethylformamide in the core layer is (25-50):
100.
4. A method for preparing a self-repairing conductive coating of aluminum tape for submarine cable armor according to claim 1, characterized in that The infusion system adopts a propulsion pump, the propulsion speed of the core layer material propulsion pump is (0.05~1) mL / h, and the propulsion speed of the shell layer material propulsion pump is (0.1~2) mL / h.
5. A method for preparing a self-repairing conductive coating of aluminum tape for submarine cable armor according to claim 1, characterized in that The conductive self-healing coating described in step 2 is composed of the following substances in percentage by mass: beaded structure fiber is 5%~10%, conductive polymer is 69%~78%, conductive filler is 6%~13%, curing agent is 4%~8%, modifier is 1%~2%, and defoaming agent is 1%~3%.
6. A method for preparing a self-repairing conductive coating of aluminum tape for submarine cable armor according to claim 1 or 5, characterized in that The conductive polymer in step 2 is any one of diethylenetriamine and modified polyethylene emulsion; the conductive filler is any one of graphene, carbon black, and carbon nanotubes; the curing agent is any one of soybean oil epoxy resin and epoxy resin; the modifier is histamine; and the defoaming agent is aminopropylmethyldiethoxysilane.
7. A method for preparing a self-repairing conductive coating of aluminum tape for submarine cable armor according to claim 1, characterized in that The heating temperature in step 2 is 35° C. to 50° C., the stirring rate is 500 rpm, and the time is 0.5 h to 1 h.
8. A method for preparing a self-repairing conductive coating of aluminum tape for submarine cable armor according to claim 1, characterized in that The cleaning in step 3 is soaking in ethanol for 2 min to 5 min, soaking in an acid solution with a pH of 4 to 5 for 1 min to 3 min, and soaking in a citric acid aqueous solution for 15 min to 30 min, wherein the mass percentage of citric acid is 5% to 10%; The acid solution in step 3 has a pH of 4-5 and is any one of a sulfuric acid solution and a nitric acid solution.
9. A method for preparing a self-repairing conductive coating of aluminum tape for submarine cable armor according to claim 1, characterized in that The immersion treatment temperature in step 4 is 35°C to 50°C, and the treatment time is 5min to 10min.
10. A method for preparing a self-repairing conductive coating of aluminum tape for submarine cable armor according to claim 1, characterized in that The heat curing time in step 5 is 30 min to 60 min, the temperature of deionized water is 50° C. to 60° C., the rinsing time is 6 min to 9 min, and the drying temperature is 60° C. to 70° C.