Manufacturing method of polymer dielectric material, chip capacitor material containing polymer dielectric material and manufacturing method of chip capacitor material
By mixing inorganic fillers and additives in a specific proportion, it is solved by solving the problem of short storage time of polymer dielectric material slurry, and achieving a chip with high dielectric constant and low dielectric loss Capacitive material, extends storage time.
Patent Information
- Application Number
- CN202410913380.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-01
AI Technical Summary
The slurry of existing polymer dielectric materials is short, easy to precipitate or cure in advance, affecting the easy processing of chip capacitor materials.
The polymer dielectric material is formed by mixing the inorganic filler, the matrix material, the first additive and the second additive with a specific ratio of the solvent by ball milling and stirring, and drying at a certain temperature to extend the storage time.
A polymer dielectric material with high dielectric constant, small dielectric loss and long storage time was prepared to ensure that the dielectric constant is between 10 and 40, the dielectric loss is less than or equal to 0.05, and the storage time is greater than or equal to 168 hours.
Smart Images

Figure CN118879160A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of capacitor technology, and in particular to a method for manufacturing a polymer dielectric material, a chip capacitor material containing the polymer dielectric material, and a method for manufacturing the same. Background Art
[0002] Polymer dielectric materials with high dielectric constant, low dielectric loss and easy processing have gradually developed into an important dielectric material in energy storage devices due to their good flexibility and ability to store charge and uniform electric field. The existing polymer dielectric material slurry is prepared from organic epoxy resin and additives. Due to the presence of additives such as curing agents, the length of its storage time will directly affect the ease of processing of chip capacitor materials. In view of this, how to extend the storage time of polymer dielectric material slurry without reducing the performance of the polymer, so that the polymer dielectric material slurry does not precipitate or solidify prematurely during storage is a technical problem that needs to be solved urgently. Summary of the invention
[0003] In view of this, the present invention provides a polymer dielectric material and a method for manufacturing the same, and a chip capacitor material containing the material, so as to manufacture a polymer dielectric material with a high dielectric constant and a long storage period.
[0004] A method for manufacturing a polymer dielectric material, characterized in that the method comprises:
[0005] Providing inorganic filler, matrix material, first auxiliary agent, second auxiliary agent and solvent;
[0006] Dissolving the inorganic filler and the first auxiliary agent in the solvent and mixing them evenly to form a first mixed liquid;
[0007] Dissolving the base material and the second auxiliary agent in the solvent, and mixing them evenly to form a second mixed liquid;
[0008] The first mixed liquid and the second mixed liquid are uniformly mixed at a weight ratio of 1:1 to 60:1 to form the polymer dielectric material.
[0009] In an embodiment of the present invention, the inorganic filler includes at least one of sodium barium titanate, barium titanate, calcium copper titanate, calcium copper titanate, strontium titanate, strontium titanate, strontium titanate, barium strontium titanate, calcium titanate, calcium titanate, barium calcium titanate, calcium barium titanate, lead zirconate titanate, sodium lead titanate, lead titanate and lead titanate.
[0010] In an embodiment of the present invention, the matrix material includes at least one of glycidyl ether epoxy resin, glycidyl ester epoxy resin, bisphenol A epoxy resin, glycidyl amine epoxy resin, alicyclic epoxy resin, epoxidized olefin compound, sugarcane polyol epoxy resin and mixed structure epoxy resin.
[0011] In an embodiment of the present invention, the first auxiliary agent includes at least one of a curing agent and a dispersant; the second auxiliary agent includes at least one of a curing agent, a dispersant, a coupling agent, a leveling agent, a defoaming agent, and a accelerator.
[0012] In an embodiment of the present invention, the solvent includes at least two of acetone, pentanone, anhydrous ethanol, butanone, cyclohexanone, isopropyl ketone, and ethyl acetate.
[0013] In an embodiment of the present invention, dissolving the inorganic filler and the first auxiliary agent in the solvent comprises:
[0014] After the inorganic filler, the first auxiliary agent and the solvent are mixed, the first mixed solution is prepared by ball milling, wherein the ball milling speed is 100 to 300 revolutions per minute and the ball milling time is 12 to 24 hours.
[0015] In an embodiment of the present invention, dissolving the base material and the second auxiliary agent in the solvent comprises:
[0016] The base material and the second auxiliary agent are dissolved in the solvent by stirring, and the stirring method adopted is at least one of ultrasonic stirring and magnetic stirring, wherein the stirring temperature is 0 to 40° C. and the stirring time is 5 to 35 minutes.
[0017] The present application also relates to a method for manufacturing a chip capacitor material, the manufacturing method comprising:
[0018] Providing a first electrode layer, a second electrode layer, and the polymer dielectric material obtained according to the method for manufacturing a polymer dielectric material according to any one of claims 1 to 5;
[0019] Applying the polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer;
[0020] The semi-cured polymer dielectric material layer is sandwiched between the first electrode layer and the second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure the semi-cured polymer dielectric material layer and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
[0021] In an embodiment of the present invention, the drying process adopts a drying temperature of 40° C. to 170° C. and a drying time of 6 to 40 hours.
[0022] The present application also relates to a chip capacitor material, and the chip capacitor material is produced by the above-mentioned chip capacitor material production method.
[0023] Among them, the chip capacitor material is a type of planar capacitor material, which is composed of a polymer dielectric material and copper foil. Its structure is that both the upper electrode and the lower electrode are copper foil electrodes, and there is a polymer dielectric material between the upper electrode and the lower electrode.
[0024] The method for preparing the polymer dielectric material of the present invention can prepare a polymer dielectric material with high dielectric constant, low dielectric loss and long storage time. The dielectric constant of the dielectric layer formed by the polymer dielectric material is 10-40, the dielectric loss is less than or equal to 0.05, and the storage time is greater than or equal to 168 hours. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic diagram of the process of manufacturing the polymer dielectric material of the present application.
[0026] Figure 2 It is a schematic diagram of the manufacturing method of the chip capacitor material of the present application. DETAILED DESCRIPTION
[0027] The following is an explanation of the implementation of the present application by means of specific embodiments. People familiar with the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification.
[0028] In the following description, reference is made to the accompanying drawings, which describe several embodiments of the present application. It should be understood that other embodiments may be used and that mechanical, structural, electrical, and operational changes may be made without departing from the spirit and scope of the present application. The following detailed description should not be considered limiting, and the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the present application.
[0029] Although the terms first, second, etc. are used herein to describe various elements in some instances, these elements should not be limited by these terms. These terms are only used to distinguish one element from another element.
[0030] Furthermore, as used in this article, the singular forms "one", "an" and "the" are intended to include plural forms as well, unless there is an indication to the contrary in the context. It should be further understood that the terms "comprise", "include" indicate the presence of features, steps, operations, elements, components, projects, kinds, and / or groups, but do not exclude the presence, occurrence or addition of one or more other features, steps, operations, elements, components, projects, kinds, and / or groups. The terms "or" and "and / or" used herein are interpreted as inclusive, or mean any one or any combination. Therefore, "A, B or C" or "A, B and / or C" means "any of the following: A; B; C; A and B; A and C; B and C; A, B and C". Only when the combination of elements, functions, steps or operations is inherently mutually exclusive in some way, will there be an exception to this definition.
[0031] Figure 1 is a schematic diagram of a process for preparing a polymer dielectric material of the present application, such as Figure 1 As shown, the method for making a polymer dielectric material includes:
[0032] Providing inorganic filler, matrix material, first auxiliary agent, second auxiliary agent and solvent;
[0033] The inorganic filler and the first auxiliary agent are dissolved in a solvent and mixed evenly to form a first mixed solution. Specifically, after the inorganic filler, the first auxiliary agent and the solvent are mixed, the first mixed solution is prepared by ball milling, wherein the ball milling speed is 100 to 300 revolutions per minute and the ball milling time is 12 to 24 hours.
[0034] The base material and the second auxiliary agent are dissolved in the solvent and mixed evenly to form a second mixed liquid. Specifically, the base material and the second auxiliary agent are dissolved in the solvent by stirring. The stirring method adopted is at least one of ultrasonic stirring and magnetic stirring, wherein the stirring temperature is 0 to 40° C. and the stirring time is 5 to 35 minutes.
[0035] The first mixed liquid and the second mixed liquid are uniformly mixed at a weight ratio of 1:1 to 60:1 to form the polymer dielectric material.
[0036] The first mixed liquid and the second mixed liquid are uniformly mixed in a weight ratio of 1:1 to 60:1, for example, 1:1, 1.5:1, 5:1, 5.5:1, 10:1, 10.5:1, 15:1, 15.5:1, 20:1, 20.5:1, 25:1, 25.5:1, 30:1, 30.5:1, 35:1, 35.5:1, 40:1, 45:1, 45.5:1, 50:1, 50.5:1, 55.5:1, 60:1;
[0037] The solid content of the polymer dielectric material is 1% to 99%, for example, 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 99%;
[0038] The viscosity of the polymer dielectric material is 1 to 500 centipoise, for example, 1 centipoise, 3 centipoise, 5 centipoise, 7 centipoise, 9 centipoise, 10 centipoise, 20 centipoise, 30 centipoise, 40 centipoise, 50 centipoise, 60 centipoise, 70 centipoise, 80 centipoise, 90 centipoise, 100 centipoise, 200 centipoise, 300 centipoise, 400 centipoise, 450 centipoise, 460 centipoise, 470 centipoise, 480 centipoise, 490 centipoise, and 500 centipoise.
[0039] The method for producing a flat polymer dielectric material of the present application can produce a polymer dielectric material with a high dielectric constant, low dielectric loss and a long storage time. The dielectric constant of the dielectric layer formed by the polymer dielectric material is 10 to 40, the dielectric loss is less than or equal to 0.05, and the storage time is greater than or equal to 168 hours.
[0040] Optionally, the inorganic filler includes at least one of sodium barium titanate, barium titanate, calcium copper titanate, calcium copper titanate, strontium titanate, strontium titanate, strontium titanate, barium strontium titanate, calcium titanate, calcium titanate, barium calcium titanate, calcium barium titanate, lead zirconate titanate, sodium lead titanate, lead titanate and lead titanate.
[0041] Optionally, the matrix material includes at least one of resins including glycidyl ether epoxy resin, glycidyl ester epoxy resin, bisphenol A epoxy resin, glycidyl amine epoxy resin, alicyclic epoxy resin, epoxidized olefin compound, sugarcane polyol epoxy resin and mixed structure epoxy resin.
[0042] Optionally, the first auxiliary agent includes at least one of a curing agent and a dispersant; and the second auxiliary agent includes at least one of a curing agent, a dispersant, a coupling agent, a leveling agent, a defoaming agent, and a accelerator.
[0043] Optionally, the solvent includes at least two of acetone, pentanone, anhydrous ethanol, butanone, cyclohexanone, isopropyl ketone, and ethyl acetate.
[0044] Figure 2 is a flow chart of a method for manufacturing a chip capacitor material of the present application. The present application also relates to a method for manufacturing a chip capacitor material, such as Figure 2 As shown, the method for making the chip capacitor material includes:
[0045] Providing a first electrode layer, a second electrode layer, and a polymer dielectric material obtained according to the method for making the polymer dielectric material;
[0046] Applying a polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer;
[0047] A semi-cured polymer dielectric material layer is sandwiched between a first electrode layer and a second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
[0048] Optionally, the drying process uses a drying temperature of 40° C. to 170° C. and a drying time of 6 to 40 hours.
[0049] Optionally, the dielectric constant of the chip capacitor material is 10-40, for example, 10, 12, 14, 16, 20, 25, 30, or 35.
[0050] Optionally, the dielectric loss of the chip capacitor material is less than or equal to 0.05.
[0051] Optionally, the dielectric layer thickness of the chip capacitor material is 1 μm to 50 μm, for example, 2 μm, 4 μm, 5 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 20 μm, 30 μm, 40 μm, or 50 μm.
[0052] Example 1
[0053] Dissolve 50% to 70% of the total mass of the first mixed solution in barium titanate and curing agent diethylenetriamine, and 1% to 5% of the total mass of the first mixed solution in a mixed solvent of anhydrous ethanol, butanone and ethyl acetate, pour the mixture into a grinding jar, and grind at a speed of 100 to 300 rpm for 12 hours to obtain a first mixed solution;
[0054] 60g of bisphenol A epoxy resin and 1% to 5% of the auxiliary agent of the total mass of the second mixed solution were dissolved in 8g of anhydrous ethanol and 32g of a mixed solvent of butanone and ethyl acetate, ultrasonically stirred at room temperature for 20 minutes, and allowed to stand for defoaming for 30 minutes to obtain a second mixed solution.
[0055] The first mixed liquid and the second mixed liquid are mixed at a weight ratio of 10:1 to obtain a polymer dielectric material.
[0056] providing a first electrode layer and a second electrode layer;
[0057] Applying the polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer;
[0058] A semi-cured polymer dielectric material layer is sandwiched between a first electrode layer and a second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
[0059] The chip capacitor material was tested and found to have a dielectric layer thickness of 41 μm, a dielectric constant of 24.58 at a frequency of 1000 Hz, and a dielectric loss of 0.0340.
[0060] Example 2
[0061] Dissolve 50% to 70% of the total mass of the first mixed solution in barium titanate and curing agent diethylenetriamine, and 1% to 5% of the total mass of the first mixed solution in a mixed solvent of anhydrous ethanol, butanone and ethyl acetate, pour the mixture into a grinding jar, and grind at a speed of 100 to 300 rpm for 12 hours to obtain a first mixed solution;
[0062] 60g of bisphenol A epoxy resin and 1% to 5% of the auxiliary agent of the total mass of the second mixed solution were dissolved in 8g of anhydrous ethanol and 32g of a mixed solvent of butanone and ethyl acetate, ultrasonically stirred at room temperature for 20 minutes, and allowed to stand for defoaming for 30 minutes to obtain a second mixed solution.
[0063] After the first mixed liquid is sealed and stored at room temperature for 12 hours, the first mixed liquid and the second mixed liquid are mixed at a weight ratio of 10:1 to obtain a polymer dielectric material.
[0064] providing a first electrode layer and a second electrode layer;
[0065] Applying the polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer;
[0066] A semi-cured polymer dielectric material layer is sandwiched between a first electrode layer and a second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
[0067] The chip capacitor material was tested and found that the dielectric layer thickness was 40 μm, the dielectric constant was measured to be 24.35 at a frequency of 1000 Hz, and the dielectric loss was 0.0356.
[0068] Example 3
[0069] Dissolve 50% to 70% of the total mass of the first mixed solution in barium titanate and curing agent diethylenetriamine, and 1% to 5% of the total mass of the first mixed solution in a mixed solvent of anhydrous ethanol, butanone and ethyl acetate, pour the mixture into a grinding jar, and grind at a speed of 100 to 300 rpm for 12 hours to obtain a first mixed solution;
[0070] 60g of bisphenol A epoxy resin and 1% to 5% of the auxiliary agent of the total mass of the second mixed solution were dissolved in 8g of anhydrous ethanol and 32g of a mixed solvent of butanone and ethyl acetate, ultrasonically stirred at room temperature for 20 minutes, and allowed to stand for defoaming for 30 minutes to obtain a second mixed solution.
[0071] After the first mixed liquid is sealed and stored at room temperature for 24 hours, the first mixed liquid and the second mixed liquid are mixed at a weight ratio of 10:1 to obtain a polymer dielectric material.
[0072] providing a first electrode layer and a second electrode layer;
[0073] Applying the polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer;
[0074] A semi-cured polymer dielectric material layer is sandwiched between a first electrode layer and a second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
[0075] The chip capacitor material was tested and found to have a dielectric layer thickness of 42 μm, a dielectric constant of 23.89 at a frequency of 1000 Hz, and a dielectric loss of 0.0345.
[0076] Example 4
[0077] Dissolve 50% to 70% of the total mass of the first mixed solution in barium titanate and curing agent diethylenetriamine, and 1% to 5% of the total mass of the first mixed solution in a mixed solvent of anhydrous ethanol, butanone and ethyl acetate, pour the mixture into a grinding jar, and grind at a speed of 100 to 300 rpm for 12 hours to obtain a first mixed solution;
[0078] 60g of bisphenol A epoxy resin and 1% to 5% of the auxiliary agent of the total mass of the second mixed solution were dissolved in 8g of anhydrous ethanol and 32g of a mixed solvent of butanone and ethyl acetate, ultrasonically stirred at room temperature for 20 minutes, and allowed to stand for defoaming for 30 minutes to obtain a second mixed solution.
[0079] After the first mixed liquid is sealed and stored at room temperature for 48 hours, the first mixed liquid and the second mixed liquid are mixed at a weight ratio of 10:1 to obtain a polymer dielectric material.
[0080] providing a first electrode layer and a second electrode layer;
[0081] Applying the polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer;
[0082] A semi-cured polymer dielectric material layer is sandwiched between a first electrode layer and a second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
[0083] The chip capacitor material was tested and found to have a dielectric layer thickness of 43 μm, a dielectric constant of 23.61 at a frequency of 1000 Hz, and a dielectric loss of 0.0350.
[0084] Example 5
[0085] Dissolve 50% to 70% of the total mass of the first mixed solution in barium titanate and curing agent diethylenetriamine, and 1% to 5% of the total mass of the first mixed solution in a mixed solvent of anhydrous ethanol, butanone and ethyl acetate, pour the mixture into a grinding jar, and grind at a speed of 100 to 300 rpm for 12 hours to obtain a first mixed solution;
[0086] 60g of bisphenol A epoxy resin and 1% to 5% of the auxiliary agent of the total mass of the second mixed solution were dissolved in 8g of anhydrous ethanol and 32g of a mixed solvent of butanone and ethyl acetate, ultrasonically stirred at room temperature for 20 minutes, and allowed to stand for defoaming for 30 minutes to obtain a second mixed solution.
[0087] After the first mixed liquid is sealed and stored at room temperature for 72 hours, the first mixed liquid and the second mixed liquid are mixed at a weight ratio of 10:1 to obtain a polymer dielectric material.
[0088] providing a first electrode layer and a second electrode layer;
[0089] Applying the polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer;
[0090] A semi-cured polymer dielectric material layer is sandwiched between a first electrode layer and a second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
[0091] The chip capacitor material was tested and found to have a dielectric layer thickness of 43 μm, a dielectric constant of 25.16 at a frequency of 1000 Hz, and a dielectric loss of 0.0369.
[0092] Example 6
[0093] Dissolve 50% to 70% of the total mass of the first mixed solution in barium titanate and curing agent diethylenetriamine, and 1% to 5% of the total mass of the first mixed solution in a mixed solvent of anhydrous ethanol, butanone and ethyl acetate, pour the mixture into a grinding jar, and grind at a speed of 100 to 300 rpm for 12 hours to obtain a first mixed solution;
[0094] 60g of bisphenol A epoxy resin and 1% to 5% of the auxiliary agent of the total mass of the second mixed solution were dissolved in 8g of anhydrous ethanol and 32g of a mixed solvent of butanone and ethyl acetate, ultrasonically stirred at room temperature for 20 minutes, and allowed to stand for defoaming for 30 minutes to obtain a second mixed solution.
[0095] After the first mixed liquid is sealed and stored at room temperature for 120 hours, the first mixed liquid and the second mixed liquid are mixed at a weight ratio of 10:1 to obtain a polymer dielectric material.
[0096] providing a first electrode layer and a second electrode layer;
[0097] Applying the polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer;
[0098] A semi-cured polymer dielectric material layer is sandwiched between a first electrode layer and a second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
[0099] The chip capacitor material was tested and found to have a dielectric layer thickness of 43 μm, a dielectric constant of 25.89 at a frequency of 1000 Hz, and a dielectric loss of 0.0373.
[0100] Example 7
[0101] Dissolve 50% to 70% of the total mass of the first mixed solution in barium titanate and curing agent diethylenetriamine, and 1% to 5% of the total mass of the first mixed solution in a mixed solvent of anhydrous ethanol, butanone and ethyl acetate, pour the mixture into a grinding jar, and grind at a speed of 100 to 300 rpm for 12 hours to obtain a first mixed solution;
[0102] 60g of bisphenol A epoxy resin and 1% to 5% of the auxiliary agent of the total mass of the second mixed solution were dissolved in 8g of anhydrous ethanol and 32g of a mixed solvent of butanone and ethyl acetate, ultrasonically stirred at room temperature for 20 minutes, and allowed to stand for defoaming for 30 minutes to obtain a second mixed solution.
[0103] After the first mixed liquid is sealed and stored at room temperature for 168 hours, the first mixed liquid and the second mixed liquid are mixed at a weight ratio of 10:1 to obtain a polymer dielectric material.
[0104] providing a first electrode layer and a second electrode layer;
[0105] Applying the polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer;
[0106] A semi-cured polymer dielectric material layer is sandwiched between a first electrode layer and a second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
[0107] The chip capacitor material was tested and found to have a dielectric layer thickness of 49 μm, a dielectric constant of 26.41 at a frequency of 1000 Hz, and a dielectric loss of 0.0395.
[0108] Example 8
[0109] Dissolve 50% to 70% of the total mass of the first mixed solution in barium titanate and curing agent diethylenetriamine, and 1% to 5% of the total mass of the first mixed solution in a mixed solvent of anhydrous ethanol, butanone and ethyl acetate, pour the mixture into a grinding jar, and grind at a speed of 100 to 300 rpm for 12 hours to obtain a first mixed solution;
[0110] 60g of bisphenol A epoxy resin and 1% to 5% of the auxiliary agent of the total mass of the second mixed solution were dissolved in 8g of anhydrous ethanol and 32g of a mixed solvent of butanone and ethyl acetate, ultrasonically stirred at room temperature for 20 minutes, and allowed to stand for defoaming for 30 minutes to obtain a second mixed solution.
[0111] After the first mixed liquid is sealed and stored at room temperature for 200 hours, the first mixed liquid and the second mixed liquid are mixed at a weight ratio of 10:1 to obtain a polymer dielectric material.
[0112] providing a first electrode layer and a second electrode layer;
[0113] Applying the polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer;
[0114] A semi-cured polymer dielectric material layer is sandwiched between a first electrode layer and a second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
[0115] The chip capacitor material was tested and found that the dielectric layer thickness was 50 μm, the dielectric constant was measured to be 26.83 at a frequency of 1000 Hz, and the dielectric loss was 0.0408.
[0116] Example 9
[0117] Dissolve 75% of the total mass of the first mixed solution in barium titanate and curing agent diethylenetriamine, and 1% to 5% of the total mass of the first mixed solution in a mixed solvent of anhydrous ethanol, butanone and ethyl acetate, pour the mixture into a grinding jar, and grind at a speed of 100 to 300 rpm for 12 hours to obtain a first mixed solution;
[0118] 60g of bisphenol A epoxy resin and 1% to 5% of the auxiliary agent of the total mass of the second mixed solution were dissolved in 8g of anhydrous ethanol and 32g of a mixed solvent of butanone and ethyl acetate, ultrasonically stirred at room temperature for 20 minutes, and allowed to stand for defoaming for 30 minutes to obtain a second mixed solution.
[0119] The first mixed liquid and the second mixed liquid are mixed at a weight ratio of 16:1 to obtain a polymer dielectric material.
[0120] providing a first electrode layer and a second electrode layer;
[0121] Applying the polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer;
[0122] A semi-cured polymer dielectric material layer is sandwiched between a first electrode layer and a second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
[0123] The chip capacitor material was tested and found to have a dielectric layer thickness of 39 μm, a dielectric constant of 32.13 at a frequency of 1000 Hz, and a dielectric loss of 0.0358.
[0124] Example 10
[0125] Dissolve 75% of the total mass of the first mixed solution in barium titanate and curing agent diethylenetriamine, and 1% to 5% of the total mass of the first mixed solution in a mixed solvent of anhydrous ethanol, butanone and ethyl acetate, pour the mixture into a grinding jar, and grind at a speed of 100 to 300 rpm for 12 hours to obtain a first mixed solution;
[0126] 60g of bisphenol A epoxy resin and 1% to 5% of the auxiliary agent of the total mass of the second mixed solution were dissolved in 8g of anhydrous ethanol and 32g of a mixed solvent of butanone and ethyl acetate, ultrasonically stirred at room temperature for 20 minutes, and allowed to stand for defoaming for 30 minutes to obtain a second mixed solution.
[0127] After the first mixed liquid was sealed and stored at room temperature for 168 hours, the first mixed liquid and the second mixed liquid were mixed at a weight ratio of 16:1 to obtain a polymer dielectric material.
[0128] providing a first electrode layer and a second electrode layer;
[0129] Applying the polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer;
[0130] A semi-cured polymer dielectric material layer is sandwiched between a first electrode layer and a second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
[0131] The chip capacitor material was tested and found to have a dielectric layer thickness of 41 μm, a dielectric constant of 33.41 at a frequency of 1000 Hz, and a dielectric loss of 0.0393.
[0132] Embodiment 11
[0133] Dissolve 75% of the total mass of the first mixed solution in barium titanate and curing agent diethylenetriamine, and 1% to 5% of the total mass of the first mixed solution in a mixed solvent of anhydrous ethanol, butanone and ethyl acetate, pour the mixture into a grinding jar, and grind at a speed of 100 to 300 rpm for 12 hours to obtain a first mixed solution;
[0134] 60g of bisphenol A epoxy resin and 1% to 5% of the auxiliary agent of the total mass of the second mixed solution were dissolved in 8g of anhydrous ethanol and 32g of a mixed solvent of butanone and ethyl acetate, ultrasonically stirred at room temperature for 20 minutes, and allowed to stand for defoaming for 30 minutes to obtain a second mixed solution.
[0135] After the first mixed liquid is sealed and stored at room temperature for 200 hours, the first mixed liquid and the second mixed liquid are mixed at a weight ratio of 16:1 to obtain a polymer dielectric material.
[0136] providing a first electrode layer and a second electrode layer;
[0137] Applying the polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer;
[0138] A semi-cured polymer dielectric material layer is sandwiched between a first electrode layer and a second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
[0139] The chip capacitor material was tested and found that the dielectric layer thickness was 45 μm, the dielectric constant was measured to be 36.40 at a frequency of 1000 Hz, and the dielectric loss was 0.0412.
[0140] Example 12
[0141] Dissolve 700 g of barium titanate, 50 g of curing agent diethylenetriamine, and 1% to 5% of the total mass of the first mixed solution in a dispersant in 40 g of anhydrous ethanol and 160 g of a mixed solvent of butanone and ethyl acetate to obtain a first mixed solution;
[0142] Dissolve 60g of bisphenol A epoxy resin and 1% to 5% of the total mass of the second mixed solution in 8g of anhydrous ethanol and 32g of a mixed solvent of butanone and ethyl acetate to obtain a second mixed solution;
[0143] The first mixed solution and the second mixed solution are mixed and poured into a grinding jar, and ground at a speed of 100 to 300 rpm for 12 hours to obtain a polymer dielectric material;
[0144] providing a first electrode layer and a second electrode layer;
[0145] Applying the polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer;
[0146] A semi-cured polymer dielectric material layer is sandwiched between a first electrode layer and a second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
[0147] The chip capacitor material was tested and found to have a dielectric layer thickness of 42 μm, a dielectric constant of 22.41 at a frequency of 1000 Hz, and a dielectric loss of 0.0386.
[0148] Example 13
[0149] Dissolve 60g of bisphenol A epoxy resin and 1% to 5% of the total mass of the second mixed solution in 8g of anhydrous ethanol and 32g of a mixed solvent of butanone and ethyl acetate to obtain a second mixed solution;
[0150] The first mixed solution and the second mixed solution are mixed and poured into a grinding jar, and ground at a rotation speed of 100 to 300 revolutions per minute for 12 hours to obtain a polymer dielectric material.
[0151] The polymer dielectric material was stored in a sealed container at room temperature for 6 hours.
[0152] providing a first electrode layer and a second electrode layer;
[0153] Applying the polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer;
[0154] A semi-cured polymer dielectric material layer is sandwiched between a first electrode layer and a second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
[0155] The chip capacitor material was tested and found to have a dielectric layer thickness of 38 μm, a dielectric constant of 19.35 at a frequency of 1000 Hz, and a dielectric loss of 0.0436.
[0156] Embodiment 14
[0157] Dissolve 60g of bisphenol A epoxy resin and 1% to 5% of the total mass of the second mixed solution in 8g of anhydrous ethanol and 32g of a mixed solvent of butanone and ethyl acetate to obtain a second mixed solution;
[0158] The first mixed solution and the second mixed solution are mixed and poured into a grinding jar, and ground at a rotation speed of 100 to 300 revolutions per minute for 12 hours to obtain a polymer dielectric material.
[0159] The polymer dielectric material was stored in a sealed container at room temperature for 12 hours.
[0160] providing a first electrode layer and a second electrode layer;
[0161] Applying the polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer;
[0162] A semi-cured polymer dielectric material layer is sandwiched between a first electrode layer and a second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
[0163] The chip capacitor material was tested and found to have a dielectric layer thickness of 39 μm, a dielectric constant of 14.32 at a frequency of 1000 Hz, and a dielectric loss of 0.0488.
[0164] Embodiment 15
[0165] Dissolve 60g of bisphenol A epoxy resin and 1% to 5% of the total mass of the second mixed solution in 8g of anhydrous ethanol and 32g of a mixed solvent of butanone and ethyl acetate to obtain a second mixed solution;
[0166] The first mixed solution and the second mixed solution are mixed and poured into a grinding jar, and ground at a rotation speed of 100 to 300 revolutions per minute for 12 hours to obtain a polymer dielectric material.
[0167] The polymer dielectric material was stored in a sealed container at room temperature for 24 hours.
[0168] providing a first electrode layer and a second electrode layer;
[0169] Applying the polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer;
[0170] A semi-cured polymer dielectric material layer is sandwiched between a first electrode layer and a second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
[0171] The chip capacitor material was tested and found to have a dielectric layer thickness of 42 μm, a dielectric constant of 10.57 at a frequency of 1000 Hz, and a dielectric loss of 0.0535.
[0172] It can be seen from the above comparative examples that if the technical solution of directly mixing the first mixed liquid and the second mixed liquid in the comparative example and then grinding to obtain the polymer dielectric material is adopted, as the storage time of the polymer dielectric material increases, the dielectric constant of the chip capacitor material containing the dielectric layer of the polymer dielectric material gradually decreases, and its dielectric loss will be greater than 0.05. If the technical solution of the polymer dielectric material obtained by grinding the first mixed liquid in the embodiment, stirring and standing the second mixed liquid, and then mixing the first mixed liquid and the second mixed liquid in a certain mass ratio is adopted, when the mass ratio of the first mixed liquid and the second mixed liquid is the same, as the storage time of the polymer dielectric material increases, the dielectric constant of the chip capacitor material containing the dielectric layer of the polymer dielectric material gradually increases, and its dielectric loss is always less than or equal to 0.05.
[0173] The dielectric layer thickness, dielectric constant, and dielectric loss parameter tables of the chip capacitor materials in the embodiments and comparative examples are as follows:
[0174]
[0175]
[0176] It can be seen from the above comparative examples that if the technical solution of directly mixing the first mixed liquid and the second mixed liquid in Examples 12-15 and then grinding to obtain the polymer dielectric material is adopted, as the storage time of the polymer dielectric material increases, the dielectric constant of the chip capacitor material containing the dielectric layer of the polymer dielectric material gradually decreases, and its dielectric loss will be greater than 0.05. If the technical solution of grinding the first mixed liquid in Examples 1-11, stirring and standing the second mixed liquid, and then mixing the first mixed liquid and the second mixed liquid in a certain mass ratio to obtain the polymer dielectric material is adopted, when the mass ratio of the first mixed liquid and the second mixed liquid is the same, as the storage time of the polymer dielectric material increases, the dielectric constant of the chip capacitor material containing the dielectric layer of the polymer dielectric material gradually increases, and its dielectric loss is always less than or equal to 0.05.
[0177] The above embodiments are merely illustrative of the principles and effects of the present application and are not intended to limit the present application. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present application. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed in the present application shall still be covered by the claims of the present application.
Claims
1. A method for preparing a polymer dielectric material, It is characterized in that The method comprises: Providing inorganic filler, matrix material, first auxiliary agent, second auxiliary agent and solvent; Dissolving the inorganic filler and the first auxiliary agent in the solvent and mixing them evenly to form a first mixed liquid; Dissolving the base material and the second auxiliary agent in the solvent, and mixing them evenly to form a second mixed liquid; The first mixed liquid and the second mixed liquid are uniformly mixed at a weight ratio of 1:1 to 60:1 to form the polymer dielectric material.
2. The method for producing a polymer dielectric material according to claim 1, It is characterized in that The inorganic filler includes at least one of sodium barium titanate, barium titanate, calcium copper titanate, calcium copper titanate, strontium titanate, strontium titanate, strontium titanate, barium strontium titanate, calcium titanate, calcium titanate, barium calcium titanate, calcium barium titanate, lead zirconate titanate, sodium lead titanate, lead titanate and lead titanate.
3. The method for producing a polymer dielectric material according to claim 1, It is characterized in that The matrix material includes at least one of glycidyl ether epoxy resin, glycidyl ester epoxy resin, bisphenol A epoxy resin, glycidyl amine epoxy resin, alicyclic epoxy resin, epoxidized olefin compound, sugarcane polyol epoxy resin and mixed structure epoxy resin.
4. The method for producing a polymer dielectric material according to claim 1, It is characterized in that The first auxiliary agent includes at least one of a curing agent and a dispersant; the second auxiliary agent includes at least one of a curing agent, a dispersant, a coupling agent, a leveling agent, a defoaming agent, and a accelerator.
5. The method for making a polymer dielectric material according to claim 1, It is characterized in that The solvent includes at least two of acetone, pentanone, anhydrous ethanol, butanone, cyclohexanone, isopropyl ketone and ethyl acetate.
6. The method for producing a polymer dielectric material according to claim 1, It is characterized in that The step of dissolving the inorganic filler and the first auxiliary agent in the solvent comprises: After the inorganic filler, the first auxiliary agent and the solvent are mixed, the first mixed solution is prepared by ball milling, wherein the ball milling speed is 100 to 300 revolutions per minute and the ball milling time is 12 to 24 hours.
7. The method for making a polymer dielectric material according to claim 1, It is characterized in that The step of dissolving the base material and the second auxiliary agent in the solvent comprises: The base material and the second auxiliary agent are dissolved in the solvent by stirring, and the stirring method adopted is at least one of ultrasonic stirring and magnetic stirring, wherein the stirring temperature is 0 to 40° C. and the stirring time is 5 to 35 minutes.
8. A method for manufacturing a chip capacitor material, It is characterized in that The method comprises: Providing a first electrode layer, a second electrode layer, and the polymer dielectric material obtained according to the method for manufacturing a polymer dielectric material according to any one of claims 1 to 5; Applying the polymer dielectric material on the surface of the first electrode layer to form a semi-cured polymer dielectric material layer on the surface of the first electrode layer; The semi-cured polymer dielectric material layer is sandwiched between the first electrode layer and the second electrode layer, and the semi-cured polymer dielectric material layer is dried to cure the semi-cured polymer dielectric material layer and adhere to the first electrode layer and the second electrode layer, thereby forming a chip capacitor material.
9. The method for manufacturing the chip capacitor material according to claim 8, It is characterized in that The drying process adopts a drying temperature of 40° C. to 170° C. and a drying time of 6 to 40 hours.
10. A chip capacitor material, It is characterized in that The chip capacitor material is obtained by the chip capacitor material manufacturing method according to claim 8 or 9.
Citation Information
Patent Citations
Preparation method of high-dielectric film
CN103242660A
Method for manufacturing high dielectric composite thin film
CN103319736A
Polymer matrix composite dielectric material and preparation method thereof
CN110684222A
Planar capacitor material and manufacturing method thereof, and manufacturing method of dielectric layer solution of planar capacitor material
CN117095953A
Paste composition and dielectric composition using the same
US20110014448A1