Fireproof flame-retardant coating for shock absorbers of high-speed rails, bullet trains and subways and preparation method of fireproof flame-retardant coating
By using cross-linking reaction technology of multi-component coatings on high-speed rail, EMU and subway shock absorbers, the problem that fire-retardant coatings in the existing technology is difficult to meet European standards, and high elongation, smoke density and thermal stability are achieved. The improvement of performance meets the fire-proof and flame-retardant needs of high-speed rail, EMU and subway.
Patent Information
- Application Number
- CN202410918160.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing technology is difficult to realize fire-resistant and flame-retardant coatings on high-speed rail, EMU and subway shock absorbers, especially it is difficult to meet the requirements of the European fire-retardant standard EN45545-2, and the smoke density of existing water-based elastic fire-retardant coatings is unstable and thermally stable. Poor performance and poor product stability.
Fire-retardant coatings including A and B are used. Component A is composed of a variety of raw materials, such as polyurethane emulsion, dehydrating agent, carbon-forming agent, titanium dioxide, smoke-repellent agent, etc. Component B is a crosslinking agent , through specific proportioning and emulsification treatment methods, a high elongation, low temperature resistance, fire-resistant and flame-retardant coating is formed, and the crosslinking agent reacts with the carboxyl group to form an imide bond, which improves the strength and toughness of the coating.
The high elongation of the coating, the smoke density reaches three-level HL3, and the thermal diffusion rate reaches three-level HL3, which is resistant to low temperatures below -40℃. The thermal stability and chemical stability of the coating are significantly improved, avoiding the oily fire-resistant coating. Environmental pollution and health risks meet the user's stability and performance requirements.
Smart Images

Figure CN118879178A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of fire-retardant coatings, and in particular relates to a fire-retardant coating for use on shock absorbers of high-speed railways, motor vehicles and subways, and a preparation method thereof. Background Art
[0002] Shock absorbers are widely used in high-speed rail, motor vehicle and subway industries, mainly to accelerate the attenuation of frame and body vibration, and to improve the smoothness of high-speed rail, motor vehicle and subway. Therefore, they play a vital role in high-speed rail, motor vehicle and subway. Since the surface of the shock absorber is mostly made of natural rubber, which is flammable, there is a complete blank in the existing technology in terms of shock absorber fire retardant coating technology, and it is difficult to meet the requirements of the European fire retardant standard EN45545-2. The water-based elastic fire retardant coating obtained by our company's prior patent CN115521699A, although the smoke density has reached the third level of smoke density HL3, but the smoke density is unstable, affected by the large changes in raw material composition, poor thermal stability, poor product stability, high defect rate, and it is difficult to meet user requirements. Summary of the invention
[0003] In order to solve the problems in the prior art, the present invention provides a fire-retardant coating and a preparation method for high-speed rail, motor vehicle and subway shock absorbers. The product performance is stable, the elongation of the coating is higher than 350%, and it is resistant to low temperatures below -40°C. The fire-retardant grade meets the requirements of EU EN45545 HL3.
[0004] The present invention solves the technical problem by adopting the following technical solutions:
[0005] The first object of the present invention is to provide a fire-retardant coating for high-speed rail, motor vehicle and subway shock absorber, characterized in that it includes two components A and B, and component A includes the following raw materials in parts by weight:
[0006]
[0007]
[0008] Component B is a cross-linking agent, and the average functionality of the cross-linking agent in reaction with carboxyl groups is 2 to 2.5;
[0009] The mass ratio of component A to component B is 19-20:1-2.
[0010] Furthermore, the crosslinking agent is a polycarbodiimide crosslinking agent, and the average functionality of the polycarbodiimide crosslinking agent with carboxyl is 2.2. The selected crosslinking agent has a low functionality with carboxyl. If the functionality is high, the crosslinking density is large, which will greatly reduce the elongation of the coating and easily break.
[0011] Furthermore, a fire-retardant coating for high-speed rail, motor vehicle and subway shock absorber is characterized in that it includes two components A and B, and component A includes the following raw materials in parts by weight:
[0012]
[0013]
[0014] Component B is a cross-linking agent, and the average functionality of the cross-linking agent in reaction with carboxyl groups is 2 to 5;
[0015] The mass ratio of component A to component B is 19-20:1-2.
[0016] Furthermore, the elongation of the high elastic emulsion is 1100-1300%.
[0017] Furthermore, the high elasticity emulsion is selected from polyurethane emulsion.
[0018] Furthermore, the silane coupling agent with a large steric hindrance group is an epoxy silane coupling agent with a large steric hindrance group.
[0019] Furthermore, the dehydrating agent is ammonium polyphosphate with a high degree of polymerization, and the degree of polymerization of the ammonium polyphosphate is greater than 1000.
[0020] Furthermore, the carbon-forming agent is micro-powdered pentaerythritol.
[0021] Furthermore, the foaming agent is melamine with a polymerization degree of 1.5 to 3.
[0022] Furthermore, the titanium dioxide is rutile titanium dioxide.
[0023] Furthermore, the smoke suppressant is zinc oxide powder.
[0024] Furthermore, the wear-resistant agent is selected from high molecular weight siloxane silicone, and the molecular weight of the siloxane silicone is greater than 600,000.
[0025] Furthermore, the high molecular weight siloxane silicone is DC51.
[0026] Furthermore, the molecular weight of the aqueous organic fluorine oligomer is 4,000 to 20,000.
[0027] Furthermore, the dispersant is a carboxylic acid-containing polymer liquid.
[0028] Furthermore, the solubility parameter of the wetting agent is 3-5.
[0029] Furthermore, the wetting agent is acetylene glycol.
[0030] Furthermore, the thickener is a polyurethane associative thickener.
[0031] Furthermore, the defoaming agent is organic silicon, and the organic silicon is DC-65.
[0032] Furthermore, the carbon black slurry is water-based carbon black slurry.
[0033] Furthermore, the emulsifying and expanding agent comprises the following raw materials in parts by weight:
[0034]
[0035]
[0036] Furthermore, the solubility parameter of the wetting agent is 3-5, the defoaming agent is silicone, and the thickener is a polyurethane associative thickener.
[0037] Furthermore, the wetting agent, defoaming agent and thickening agent selected in the emulsifying and expanding agent are consistent with the wetting agent, defoaming agent and thickening agent in component A.
[0038] Furthermore, the emulsified expansion agent is emulsified before preparing component A. Expanded graphite powder is difficult to wet and has a large particle size. The emulsion has poor adhesion to it and is easy to fall off, thereby affecting the strength of the coating. The expanded graphite is emulsified before preparing component A to improve its wettability and adjust the strength of the coating.
[0039] Furthermore, the emulsified expansion agent is selected from expanded graphite after emulsification treatment with an expansion rate of more than 120%.
[0040] The second object of the present invention is to provide a method for preparing a fire retardant coating for high-speed rail, motor vehicle and subway shock absorber, characterized in that it comprises the following steps:
[0041] 1) Preparation of emulsifying agent
[0042] Heat deionized water to 60°C, add low solubility parameter wetting agent, defoaming agent and swelling agent under stirring, accelerate stirring for 20 to 30 minutes, then slow down stirring, and add thickener until stirring is uniform;
[0043] 2) Preparation of component A
[0044] The weighed deionized water, dispersant, wetting agent, defoamer, industrial alcohol and wear-resistant agent are mixed and stirred, and after being evenly mixed, a foaming agent is added, and then a dehydrating agent, a carbon forming agent, titanium dioxide and a smoke suppressant are added under stirring, and after the powder is completely dissolved, the stirring speed is increased and stirred at high speed for 25 to 35 minutes; then the speed is reduced and a thickener, an emulsified expansion agent obtained in step 1), a carbon black slurry, an aqueous organic fluorine oligomer, an ultra-low Tg carboxyl-containing acrylic emulsion, and a high elasticity emulsion are added under stirring, and stirring is continued for 20 to 30 minutes to obtain component A;
[0045] 3) The component A obtained in step 2) and the component B obtained by weighing the cross-linking agent are separately stored for later use to form a fire-retardant coating.
[0046] Furthermore, the stirring speed during the coating preparation is 600-1200 r / min.
[0047] Furthermore, the wetting agent, defoaming agent and thickening agent used in step 1) are the same as the wetting agent, defoaming agent and thickening agent in component A of step 2).
[0048] Component A and component B are stored separately, and before use, component A and component B are mixed in a mass ratio of 19-20:1-2, and stirred evenly before use. The fire-retardant coating of the present invention needs to be baked at 95° C. for 1.5 hours when used.
[0049] After the A component is mixed with the B component, the neutralizer in the A component volatilizes under the baking condition, and the carboxyl group of the ultra-low Tg acrylic emulsion with carboxyl groups is revealed. The crosslinking agent in the B component reacts with the carboxyl group in the A component and the silane coupling agent with a large steric hindrance group. The polycarbodiimide crosslinking agent is a compound containing multiple carbon-nitrogen double bonds, which can react with the carboxyl group to form an imide bond. In the reaction, the carbon-nitrogen double bond of the polycarbodiimide crosslinking agent reacts with the carboxyl group to form an intermediate, and then the intermediate undergoes an internal condensation reaction to form an imide bond. It is this bond that forms a very strong crosslinking structure. At the same time, the crosslinking agent in the B component reacts with the silane coupling agent with a large steric hindrance group to consume the remaining hydrophilic carboxyl groups, so that the carboxyl groups in the ultra-low Tg acrylic emulsion with carboxyl groups and the free hydrophilic carboxyl groups in the coating are completely consumed, which can greatly improve the strength, toughness, heat resistance, chemical stability and corrosion resistance of the coating.
[0050] Compared with the prior art, the beneficial technical effects of the present invention are:
[0051] The present invention studies the composition of the coating components A and B so that the two components A and B react after mixing to produce excellent fire retardancy and high elongation and smoke suppression. When the coating thickness is 300um, the elongation reaches more than 350%, and the highest reaches 500%; when the coating thickness reaches more than 300um, the smoke density reaches level 3 HL3, and the heat diffusion rate reaches level 3 HL3; it is resistant to low temperatures below -40°C.
[0052] The present invention combines an epoxy silane coupling agent with a large steric hindrance with an ultra-low Tg carboxyl acrylic emulsion. The epoxy silane coupling agent is used as a crosslinking agent and an adhesion promoter. The presence of its own large steric hindrance group greatly reduces the reaction rate of the epoxy group and the carboxyl group at room temperature. The thermal stability is good. After being placed in a 50°C environment for about 20 days, the coating performance is basically unchanged. In addition, the epoxy silane coupling agent with a large steric hindrance is combined with an ultra-low Tg carboxyl acrylic emulsion to improve the solvent resistance, impact resistance, and scratch resistance of the coating; the appearance, weather resistance, and durability are outstanding; the material adhesion is good in wet and dry states; and the gloss retention rate is high after aging.
[0053] The present invention combines four materials, catalytic dehydrating agent, foaming agent, carbon forming agent and expansion agent, into an expansion system, uses zinc oxide as a smoke suppressant, and adds dispersant, wetting agent, thickener and defoaming agent to improve the storage stability and construction performance of the coating, and uses ultra-high molecular weight organosilicon as a wear-resistant agent to improve the wear resistance of the coating; the aqueous organic fluorine oligomer with a molecular weight of 4000 to 20000 plays a sliding role between the emulsions with large molecular weights, which greatly improves the fatigue resistance of the coating. According to the actual product testing by customers, the fatigue resistance has passed the fatigue acceleration test of the sample for more than 10,000 times, and the product fatigue test has passed 600,000 times under a weight of 9 tons, and there is no abnormality on the surface of the coating. The present invention avoids the need to add a large amount of organic solvents in the preparation of most oily fire retardant coatings in the prior art, which easily causes environmental pollution during preparation and construction, affecting the health of the constructors, and is non-toxic, pollution-free, environmentally friendly and has good storage stability.
[0054] Compared with patent CN115521699A, the present invention greatly enhances the strength and adhesion of the coating by adding an epoxy silane coupling agent with large steric hindrance, and adjusts the ratio of the epoxy silane coupling agent with large steric hindrance to raw materials such as ultra-low Tg carboxyl acrylic emulsion. The epoxy silane coupling agent with large steric hindrance is used as a cross-linking agent and an adhesion promoter at the same time, and the expansion agent after emulsification pretreatment greatly enhances the fatigue resistance of the coating, and rapidly reduces the smoke density and thermal diffusion rate, so that the product performance is more stable.
[0055] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 The diagram is a state diagram before and after the stretching test of Example 2 of a fire-retardant coating for shock absorbers of high-speed railways, motor vehicles and subways according to the present invention (the left side is before stretching, and the right side is after stretching);
[0057] Figure 2 This is a state diagram of Example 3 of a fire-retardant coating for high-speed rail, motor vehicle and subway shock absorber of the present invention before and after stretching 500% (the left side is before stretching, and the right side is after stretching);
[0058] Figure 3 This is a state diagram before and after burning during the smoke density test of Example 2 of the fire-retardant coating for high-speed railways, motor vehicles and subway shock absorbers of the present invention. DETAILED DESCRIPTION
[0059] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the following embodiments are only exemplary illustrations and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope of protection that the present invention is intended to protect.
[0060] In addition, unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0061] Embodiment 1:
[0062] A fire-retardant coating for shock absorbers of high-speed railways, motor vehicles and subways, comprising two components, A and B. Component A comprises the following raw materials:
[0063]
[0064]
[0065] Component B is polycarbodiimide crosslinking agent, 6.25g.
[0066] The polyurethane emulsion with an elongation of 1200% is selected.
[0067] A method for preparing a fire-retardant coating for high-speed rail, motor vehicle and subway shock absorber comprises the following steps:
[0068] 1) Preparation of expanded graphite emulsified semi-finished products
[0069] Heat 36.2g of deionized water to 60°C, and add 2.5g of a wetting agent with a solubility parameter of 4, 0.3g of Corning DC-65, and 60g of expanded graphite at a stirring speed of 600r / min. Accelerate to 1200r / min and stir for 20 to 30min, then reduce the speed to 600r / min and continue stirring. Add 1g of a polyurethane thickener until the mixture is evenly stirred to obtain an expanded graphite emulsified semi-finished product.
[0070] 2) Preparation of component A
[0071] The raw materials are weighed according to the above ratio, and the weighed deionized water, Digo 760W, acetylene glycol wetting agent, Corning DC-65, industrial alcohol, and silicone wear resistant agent are mixed and stirred at 1000r / min for 25min. After the mixture is evenly mixed, melamine resin is added, and then ammonium polyphosphate, micro-powder pentaerythritol, titanium dioxide, and micro-powder zinc oxide are added under stirring at 600r / min. After the powder is completely dissolved, the stirring speed is increased to 1200r / min and stirred at high speed for 25 to 35min; then the speed is reduced to 600r / min, and a polyurethane thickener, the expanded graphite emulsified semi-finished product obtained in step 1), an aqueous carbon black slurry, an aqueous organic fluorine oligomer, an ultra-low Tg carboxyl-containing acrylic emulsion, and an elongation of 1200% are added under stirring, and stirring is continued for 20 to 30min to obtain component A;
[0072] 3) The component A obtained in step 2) and the component B obtained by weighing the polycarbodiimide cross-linking agent are separately stored for later use to form a fire-retardant coating.
[0073] Before construction, the prepared components A and B are weighed according to the mass ratio and then mixed, and stirred at 600 r / min for 10 to 15 minutes to obtain a flame retardant coating.
[0074] Embodiment 2:
[0075] A fire-retardant coating for shock absorbers of high-speed railways, motor vehicles and subways, comprising two components, A and B. Component A comprises the following raw materials:
[0076]
[0077] Component B is polycarbodiimide crosslinking agent, 5.88g.
[0078] A method for preparing a fire-retardant coating for high-speed rail, motor vehicle and subway shock absorbers is the same as that in Example 1.
[0079] Embodiment 3:
[0080] A fire-retardant coating for shock absorbers of high-speed railways, motor vehicles and subways, comprising two components, A and B. Component A comprises the following raw materials:
[0081]
[0082]
[0083] Component B is polycarbodiimide crosslinking agent, 5.26g.
[0084] A method for preparing a fire-retardant coating for high-speed rail, motor vehicle and subway shock absorbers is the same as that in Example 1.
[0085] Comparative Example 1:
[0086] The formula of the fire retardant coating of Example 3 in patent CN115521699A is selected, and the preparation method is the same as patent CN115521699A.
[0087] Comparative Example 2:
[0088] A fire-retardant coating for shock absorbers of high-speed railways, motor vehicles and subways, comprising two components, A and B. Component A comprises the following raw materials:
[0089]
[0090]
[0091] Component B is polycarbodiimide crosslinking agent, 5.26g.
[0092] A method for preparing a fire-retardant coating for high-speed rail, motor vehicle and subway shock absorbers is the same as that in Example 1.
[0093] Experimental example:
[0094] The main properties of the fire-retardant coatings prepared in the embodiments and comparative examples were tested, and the test results are shown in Table 1.
[0095] Table 1 Main performance indicators of high elastic water-based fire retardant coatings in various embodiments
[0096]
[0097]
[0098]
[0099] Through the testing of various embodiments and comparative examples, it can be seen that the coatings of various embodiments of the present invention have good adhesion. Figure 1 The coating of Example 2 of the present invention is stretched to more than 360% and maintained for 10 seconds without cracks, and the maximum elongation can reach more than 540%. After the tensile fracture, the fault is flat, without warping, curling, or falling off. Figure 3, the coating of Example 2 of the present invention is applied to the sample until the coating thickness reaches more than 300um. After the sample is burned at 600-800℃, the sample is basically unchanged. The coating plays a good protective role on the sample. The smoke density is less than 85DS, reaching the third level HL3; the thermal diffusion rate is less than 25kW / m 2 , all reaching level 3 HL3. The products of the embodiments of the present invention have good performance, can well meet the requirements of elongation and high fatigue resistance of shock absorbers in the prior art, and avoid the phenomenon of easy cracking after long-term use.
[0100] Compared with the embodiments of the present application, the patent CN115521699A does not add epoxy silane with large steric hindrance, and adjusts the composition ratio of each raw material. Although the smoke density can reach the third level of smoke density requirement, the smoke density is very unstable and the average smoke density is relatively high; the thermal diffusion rate is significantly improved compared with the embodiments of the present invention, and only reaches the second level of thermal diffusion rate requirement. This is mainly because after the epoxy silane with large steric hindrance is added, the reaction rate of the epoxy group and the carboxyl group at room temperature is reduced, and the thermal stability is better. In addition, since the high elastic emulsion has a great influence on the smoke density and thermal diffusion rate of the coating, the change of the addition amount makes the performance of the coating very unstable. The present invention adds epoxy silane with large steric hindrance and adjusts the ratio of epoxy silane with large steric hindrance to the high elastic emulsion, and adjusts the elongation of the high elastic emulsion to 1100-1300%, so that the smoke density and thermal diffusion rate of the coating are more stable. The strength of the coating has decreased to a certain extent, and the adhesion of the coating is slightly poor. This is mainly because the expanded graphite is replaced with an emulsified expander, and the expanded graphite is emulsified before application, which improves the wettability and better adhesion.
[0101] After changing the addition amount of the high elastic emulsion in Comparative Example 2, the smoke density and thermal diffusion rate increased rapidly, and could only meet the requirements of EN45545-2:2020HL2. It can be seen that although the addition of epoxy silane with ultra-large steric hindrance enhances the stability of the coating, when the addition amount of the high elastic emulsion is greater than 50% of the mass of component A, it still has a great influence on the elongation, smoke density and thermal diffusion performance of the coating.
[0102] The serial numbers of the above embodiments of the present invention are only for description and do not represent the advantages or disadvantages of the embodiments.
[0103] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.
Claims
1. A fire retardant coating for shock absorbers of high-speed railways, motor vehicles and subways, characterized in that: It includes two components, A and B. Component A includes the following raw materials in parts by weight: Component B is a cross-linking agent, and the average functionality of the cross-linking agent in reaction with carboxyl groups is 2 to 5; The mass ratio of component A to component B is 19-20:1-2.
2. The fire-retardant coating for shock absorbers of high-speed railways, motor vehicles and subways as claimed in claim 1, characterized in that: The crosslinking agent is a polycarbodiimide crosslinking agent, and the average functionality of the polycarbodiimide crosslinking agent in reaction with carboxyl is 2.
2. The selected crosslinking agent has a low functionality in reaction with carboxyl. If the functionality is high, the crosslinking density is large, which will greatly reduce the elongation of the coating and easily cause fracture.
3. A fire retardant coating for high-speed rail, motor vehicle and subway shock absorber according to claim 1, characterized in that: It includes two components, A and B. Component A includes the following raw materials in parts by weight: Component B is a cross-linking agent, and the average functionality of the cross-linking agent in reaction with carboxyl groups is 2 to 5; The mass ratio of component A to component B is 19-20:1-2.
4. A fire retardant coating for shock absorbers of high-speed railways, motor vehicles and subways as claimed in claim 1 or 3, characterized in that: The elongation of the high elastic emulsion is 1100-1300%.
5. A fire-retardant coating for shock absorbers of high-speed railways, motor vehicles and subways as claimed in claim 1 or 3, characterized in that: The anti-wear agent is selected from high molecular weight siloxane silicone, and the molecular weight of the siloxane silicone is greater than 600,000.
6. A fire-retardant coating for shock absorbers of high-speed railways, motor vehicles and subways as claimed in claim 1 or 3, characterized in that: The molecular weight of the aqueous organic fluorine oligomer is 4,000 to 20,000.
7. A fire-retardant coating for shock absorbers of high-speed railways, motor vehicles and subways as claimed in claim 1 or 3, characterized in that: The emulsifying and expanding agent comprises the following raw materials in parts by weight:
8. The fire-retardant coating for shock absorbers of high-speed railways, motor vehicles and subways as claimed in claim 7, characterized in that: The wetting agent, defoaming agent and thickening agent selected in the emulsifying and expanding agent are consistent with the wetting agent, defoaming agent and thickening agent in component A.
9. The fire-retardant coating for shock absorbers of high-speed railways, motor vehicles and subways as claimed in claim 7, characterized in that: The emulsified expander is emulsified before preparing component A.
10. A method for preparing a fire-retardant coating for high-speed railways, motor vehicles and subway shock absorbers according to any one of claims 1 to 9, characterized in that: The following steps are involved: 1) Preparation of emulsifying agent Heat deionized water to 60°C, add low solubility parameter wetting agent, defoaming agent and swelling agent under stirring, accelerate stirring for 20 to 30 minutes, then slow down stirring, and add thickener until stirring is uniform; 2) Preparation of component A The weighed deionized water, dispersant, wetting agent, defoamer, industrial alcohol and wear-resistant agent are mixed and stirred, and after being evenly mixed, a foaming agent is added, and then a dehydrating agent, a carbon forming agent, titanium dioxide and a smoke suppressant are added under stirring, and after the powder is completely dissolved, the stirring speed is increased and stirred at high speed for 25 to 35 minutes; then the speed is reduced and a thickener, an emulsified expansion agent obtained in step 1), a carbon black slurry, an aqueous organic fluorine oligomer, an ultra-low Tg carboxyl-containing acrylic emulsion, and a high elasticity emulsion are added under stirring, and stirring is continued for 20 to 30 minutes to obtain component A; 3) The component A obtained in step 2) and the component B obtained by weighing the cross-linking agent are separately stored for later use to form a fire-retardant coating.
Citation Information
Patent Citations
Spraying polyurethane rigid foam and preparation method thereof
CN104558483A
Multifunctional water-based paint and preparation method thereof
CN114213912A
Water-based elastic fireproof coating based on soft base material and preparation method of water-based elastic fireproof coating
CN115521699A