Preparation method of low-odor water-white tackifying resin as well as product and application of low-odor water-white tackifying resin
By vacuum distillation, esterification and vegetable oil modification reaction of rosin, combined with the use of antioxidants, the problem of oxidation and odor of water-white tackifying resin at high temperatures is solved. The obtained low-odor water-white tackifying resin is suitable for sanitary products. It has good thermal stability and weather resistance.
Patent Information
- Application Number
- CN202411112178.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-01
AI Technical Summary
Traditional water-white tackifying resins are prone to oxidation, produce odor and discoloration at high temperatures, resulting in limited application in the field of sanitary products, and existing modification methods have failed to effectively solve the odor problem.
After vacuum distillation of the rosin, a catalyst, unsaturated acid and polyol were added for esterification, then vegetable oil was added for modification, and finally an antioxidant was added to obtain a low-odor water-white tackifying resin. The process involves two esterification reactions and vegetable oil modification steps, the entire process being carried out under nitrogen protection.
The obtained water-white tackifying resin has good thermal stability, weather resistance, low odor and light color. It is suitable for the field of sanitary products, and simplifies the preparation process and reduces costs.
Smart Images

Figure BDA0004992551160000041 
Figure BDA0004992551160000051 
Figure BDA0004992551160000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rosin deep processing, and particularly relates to a preparation method of a low-odor water-white tackifying resin, a product thereof and an application thereof. Background Art
[0002] Rosin is an important natural product and a renewable resource. It is widely used in adhesives, inks, coatings, electronics and other fields. However, rosin has carboxyl groups and conjugated double bonds, which have certain reactivity and have great defects in application, such as high acid value, strong odor and poor thermal stability. In order to expand the use of rosin, it needs to be modified.
[0003] Water-white tackifying resin is a product modified from rosin. It is an important component of pressure-sensitive adhesives and gives them excellent bonding properties. However, traditional water-white tackifying resins, which are made by high-temperature esterification of refined rosin and polyols, are easily oxidized by air, have poor heat resistance, and are prone to odor and discoloration at high temperatures, which limits the application of pressure-sensitive adhesives containing water-white tackifying resins.
[0004] In the field of sanitary products (such as sanitary napkins, diapers, medical products, and pet products), pressure-sensitive adhesives are required to have light color and low odor in addition to good bonding properties.
[0005] In order to reduce the color of water-white tackifying resin, a Chinese patent with publication number CN110437743B discloses a production process of water-white tackifying resin, including: a) crushing the first-grade rosin of Masson pine into a refined melting pot and melting it with a second-level firepower; b) removing the heavy oil remaining in the melted rosin, and then atomizing it at high temperature to obtain refined rosin; c) collecting the atomized refined rosin into a storage pot by vacuum; d) sucking the collected refined rosin into a reactor, first adding light-colored rosin and acrylic acid for addition reaction; then adding a catalyst and a polyol for esterification reaction to obtain a water-white tackifying resin. However, this technical solution adopts a fully enclosed operation, and the preparation process is relatively cumbersome.
[0006] A Chinese patent with publication number CN115746710A discloses a method for preparing a high-stability water-white tackifying resin, which comprises melting common rosin and performing negative pressure vacuum distillation to obtain refined rosin; adding 0.05wt%-0.2wt% of a palladium-carbon catalyst accounting for the total amount of the refined rosin at 190°C-210°C to carry out a normal pressure disproportionation hydrogenation reaction with the refined rosin; adding 0.5wt%-1.5wt% of fumaric acid accounting for the total amount of the refined rosin to carry out an addition reaction, the reaction temperature is 200°C-210°C, the reaction time is 1.5-2.5h, and then an esterification reaction is carried out to obtain a resin; however, the technical solution also uses polyols for esterification, and the odor problem of the water-white tackifying resin is not solved. The application of pressure-sensitive adhesives containing the water-white tackifying resin in the field of sanitary products is limited, so it is of great significance to develop a low-odor water-white tackifying resin. Summary of the invention
[0007] The present invention aims to solve the problem that the water-white tackifying resin in the prior art is easily oxidized by air, has poor heat resistance, and is prone to produce odor and discoloration at high temperatures, resulting in limited application of pressure-sensitive adhesives containing the water-white tackifying resin in the field of sanitary products. The present invention provides a preparation method of a low-odor water-white tackifying resin, a product thereof, and an application thereof. The water-white tackifying resin obtained by the preparation method provided by the present invention has the advantages of good thermal stability, good weather resistance, low volatility, low odor, and light color.
[0008] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0009] The first aspect of the present invention provides a method for preparing a low-odor water-whitening tackifying resin, comprising the following steps:
[0010] S1, melting rosin and vacuum distilling to obtain refined rosin;
[0011] S2, heating and melting the refined rosin, adding a catalyst, an unsaturated acid, and a polyol, raising the temperature to carry out a first esterification reaction, cooling after the first esterification reaction, and adding vegetable oil for a modification reaction;
[0012] S3, after the modification reaction is completed, polyol is added again and the temperature is raised to carry out a second esterification reaction;
[0013] S4. After the second esterification reaction is completed, washing, dehydration, cooling, and antioxidants are added to obtain the low-odor water-white tackifying resin.
[0014] Preferably, the preparation method is carried out under nitrogen protection throughout the entire process.
[0015] Preferably, step S1 specifically comprises: crushing the rosin into a two-necked distillation flask with a thermometer, heating it to 230-250° C. to melt it, and collecting the main fraction at 180-250° C. under vacuum to obtain the refined rosin.
[0016] Preferably, step S2 is specifically as follows: putting the refined rosin into a reaction bottle and heating it to melt it, adding a catalyst and an unsaturated acid to carry out an addition reaction; after the addition reaction is completed, adding a polyol, raising the temperature to carry out a first esterification reaction, cooling after the first esterification reaction is completed, and adding vegetable oil to carry out a modification reaction.
[0017] Preferably, the temperature of the addition reaction is 180-200° C. and the time is 50-70 min.
[0018] Preferably, the temperature of the first esterification reaction and the second esterification reaction is 265-285° C., and the time is 4-7 hours.
[0019] Preferably, the temperature of the first esterification reaction is 275° C. and the time is 6 hours.
[0020] Preferably, the temperature of the second esterification reaction is 275° C. and the time is 5 hours.
[0021] Preferably, the modification reaction is carried out at a temperature of 220-240° C. and a time of 0.5-1.5 h.
[0022] Preferably, step S4 is specifically as follows: after the second esterification reaction is completed, water vapor is introduced for washing for 1-3 hours, the steam is stopped, vacuum is drawn for 1-3 hours, and after cooling to 200-220° C., an antioxidant is added to obtain the low-odor water-white tackifying resin.
[0023] Preferably, the low-odor water-white tackifying resin comprises the following components in parts by weight: 900-1100 parts of refined rosin, 5-25 parts of vegetable oil, 5-45 parts of unsaturated acid, 70-135 parts of polyol, 2-5 parts of catalyst and 3-10 parts of antioxidant.
[0024] Preferably, the rosin is selected from at least one of horsetail rosin, wetland rosin, Caribbean rosin, Indonesian rosin, tall oil rosin, hydrogenated rosin and disproportionated rosin.
[0025] More preferably, the rosin is selected from at least one of horsetail rosin and wetland rosin.
[0026] Preferably, the unsaturated acid is a monobasic unsaturated acid and / or a dibasic unsaturated acid; the monobasic unsaturated acid is not specifically limited, and examples thereof include at least one of acrylic acid, oleic acid, fumaric acid, maleic anhydride or methacrylic acid; the dibasic unsaturated acid is not specifically limited, and examples thereof include at least one of malonic acid, adipic acid and itaconic acid.
[0027] Preferably, the catalyst is a well-known esterification reaction catalyst, without specific limitation, and may include at least one of acetic acid, p-toluenesulfonic acid, methanesulfonic acid, hypophosphorous acid, sulfuric acid, boric acid, phosphite, triphenyl phosphite, magnesium oxide, calcium oxide, magnesium sulfate, calcium sulfate, tricalcium phosphate and calcium hypophosphite.
[0028] Preferably, the vegetable oil is selected from at least one of tung oil, zelkova oil, castor oil, soybean oil, linseed oil and refined soybean oil.
[0029] More preferably, the vegetable oil is linseed oil and / or soybean oil.
[0030] Further preferably, the weight ratio of linseed oil to soybean oil is 1-3:1, preferably 2:1.
[0031] Preferably, the polyol is selected from at least one of a diol, a triol and a tetraol.
[0032] Preferably, the diol is selected from at least one of ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol and neopentyl glycol.
[0033] Preferably, the triol is selected from at least one of glycerol, trimethylolethane and trimethylolpropane.
[0034] Preferably, the tetrahydric alcohol is selected from at least one of pentaerythritol and dipropylene glycol.
[0035] More preferably, the polyol in step S2 is pentaerythritol; and the polyol in step S3 is glycerol.
[0036] Further preferably, the weight ratio of pentaerythritol to glycerol is 1-5:1.
[0037] Preferably, the antioxidant is selected from at least one of DTBHQ (2,5-di-tert-butylhydroquinone), antioxidant 565 (4-[(4,6-dioctylthio-1,3,5-triazine-2-yl)amino]-2,6-di-tert-butylphenol), antioxidant 1010 (pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate), BHT (2,6-di-tert-butyl-p-cresol) and TNPP (triphenyl phosphite).
[0038] The second aspect of the present invention provides a low-odor water-whitening tackifying resin obtained by the above preparation method.
[0039] The third aspect of the present invention provides a use of the low-odor water-white tackifying resin obtained by the above preparation method in the preparation of a pressure-sensitive adhesive.
[0040] A fourth aspect of the present invention provides a pressure-sensitive adhesive comprising the low-odor water-whitening tackifying resin obtained by the above preparation method.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] 1. The water-white tackifying resin obtained by the present invention sequentially reacts with addition, first esterification, vegetable oil modification and second esterification, has light color and good thermal stability, and reduces the generation of volatiles.
[0043] 2. The present invention adopts a specific vegetable oil modification step, and the obtained water-white tackifying resin has not only low odor at high temperature, but also good aging resistance.
[0044] 3. The water-white tackifying resin obtained by the present invention can be used in the field of sanitary products.
[0045] 4. The preparation method provided by the present invention is simple and low in cost. DETAILED DESCRIPTION
[0046] The present invention is further explained below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0047] In the following examples, unless otherwise specified, all raw materials used were commercially available or prepared by conventional methods in the art.
[0048] The preparation method of the refined rosin in the examples and comparative examples of the present invention is as follows: 1000g of Masson pine is crushed and placed in a two-necked distillation flask (2L) with a thermometer, the temperature is raised to 240°C and kept for 0.5h, and the main fraction at 180-250°C is collected under vacuum to obtain the refined rosin.
[0049] The formula composition of the low odor water-white tackifying resin in the examples of the present invention and the comparative examples is shown in Table 1:
[0050] Table 1
[0051]
[0052]
[0053] Example 1
[0054] A method for preparing a low-odor water-white tackifying resin (nitrogen protection throughout the process):
[0055] S1, preparing refined rosin;
[0056] S2. Accurately weigh the refined rosin, crush it, and put it into the reaction bottle, heat it to 190°C to melt it; add 4,4'-thiobis(6-tert-butyl-3-methylphenol) and fumaric acid to carry out addition reaction at a temperature of 1 hour; after the addition reaction, add pentaerythritol, gradually heat it to 275°C to carry out the first esterification reaction at a temperature of 6 hours; after the first esterification reaction, cool it to 230°C, add linseed oil to carry out modification reaction at a temperature of 1 hour;
[0057] S3. After the modification reaction is completed, glycerol is added and the temperature is gradually raised to 275°C for a second esterification reaction for 5 hours;
[0058] S4. When the acid value of the second esterification reaction is less than 12 mgKOH / g, water vapor is introduced for washing for 2 hours, the steam is stopped and vacuum is drawn for 2 hours, the mixture is cooled to 210° C., 2,5-di-tert-butylhydroquinone is added, and the mixture is stirred evenly to obtain the low-odor water-white tackifying resin.
[0059] Example 2
[0060] A method for preparing a low-odor water-white tackifying resin (nitrogen protection throughout the process):
[0061] S1, preparing refined rosin;
[0062] S2. Accurately weigh the refined rosin, crush it, and put it into the reaction bottle, heat it to 190°C to melt it; add 4,4'-thiobis(6-tert-butyl-3-methylphenol), malonic acid, and pentaerythritol, gradually heat it to 275°C to carry out the first esterification reaction for 6 hours; after the first esterification reaction, cool it to 230°C, add soybean oil and carry out the modification reaction for 1 hour;
[0063] S3, same as S3 in Example 1;
[0064] S4. Same as S4 in Example 1.
[0065] Example 3
[0066] A method for preparing a low-odor water-white tackifying resin (nitrogen protection throughout the process):
[0067] S1, preparing refined rosin;
[0068] S2. Accurately weigh the refined rosin, crush it, and put it into the reaction bottle, heat it to 190°C to melt it; add 4,4'-thiobis(6-tert-butyl-3-methylphenol), fumaric acid, and maleic anhydride to carry out heat preservation addition reaction for 1 hour; after the addition reaction, add pentaerythritol, gradually heat it to 275°C to carry out heat preservation first esterification reaction for 6 hours; after the first esterification reaction, cool it to 230°C, add castor oil to carry out heat preservation modification reaction for 1 hour;
[0069] S3, same as S3 in Example 1;
[0070] S4. Same as S4 in Example 1.
[0071] Example 4
[0072] A method for preparing a low-odor water-white tackifying resin (nitrogen protection throughout the process):
[0073] S1, preparing refined rosin;
[0074] S2. Accurately weigh the refined rosin, crush it, and put it into the reaction bottle, heat it to 190°C to melt it; add 4,4'-thiobis(6-tert-butyl-3-methylphenol) and fumaric acid to carry out addition reaction for 1 hour; after the addition reaction, add pentaerythritol, gradually heat it to 275°C to carry out the first esterification reaction for 6 hours; after the first esterification reaction, cool it to 230°C, add tung oil to carry out modification reaction for 0.5 hours;
[0075] S3, same as S3 in Example 1;
[0076] S4. Same as S4 in Example 1.
[0077] Example 5
[0078] A method for preparing a low-odor water-white tackifying resin (nitrogen protection throughout the process):
[0079] S1, preparing refined rosin;
[0080] S2. Accurately weigh the refined rosin, crush it, and put it into the reaction bottle, heat it to 190°C to melt it; add 4,4'-thiobis(6-tert-butyl-3-methylphenol) and fumaric acid to carry out addition reaction at a temperature of 1 hour; after the addition reaction, add pentaerythritol, gradually heat it to 275°C to carry out the first esterification reaction at a temperature of 6 hours; after the first esterification reaction, cool it to 230°C, add linseed oil and soybean oil to carry out modification reaction at a temperature of 1 hour;
[0081] S3, same as S3 in Example 1;
[0082] S4. Same as S4 in Example 1.
[0083] Example 6
[0084] A method for preparing a low-odor water-white tackifying resin (nitrogen protection throughout the process):
[0085] S1, preparing refined rosin;
[0086] S2. Accurately weigh the refined rosin, crush it, and put it into the reaction bottle, heat it to 190°C to melt it; add 4,4'-thiobis(6-tert-butyl-3-methylphenol) and acrylic acid to carry out addition reaction at a temperature of 1 hour; after the addition reaction, add pentaerythritol, gradually heat it to 275°C to carry out the first esterification reaction at a temperature of 6 hours; after the first esterification reaction, cool it to 230°C, add linseed oil to carry out modification reaction at a temperature of 1 hour;
[0087] S3, same as S3 in Example 1;
[0088] S4. Same as S4 in Example 1.
[0089] Comparative Example 1
[0090] A method for preparing a low-odor water-white tackifying resin (nitrogen protection throughout the process):
[0091] S1, preparing refined rosin;
[0092] S2. Accurately weigh the refined rosin, crush it, and put it into the reaction bottle, heat it to 190°C to melt it; add 4,4'-thiobis(6-tert-butyl-3-methylphenol) and acrylic acid to carry out addition reaction for 1 hour; after the addition reaction, add pentaerythritol, gradually heat it to 275°C to carry out the first esterification reaction for 6 hours; after the first esterification reaction, cool it to 230°C;
[0093] S3, same as S3 of Example 6;
[0094] S4. Same as S4 in Example 6.
[0095] Comparative Example 2
[0096] A method for preparing a low-odor water-white tackifying resin (nitrogen protection throughout the process):
[0097] S1, preparing refined rosin;
[0098] S2. Accurately weigh the refined rosin, crush it, and put it into the reaction bottle, heat it to 190°C to melt it; add 4,4'-thiobis(6-tert-butyl-3-methylphenol) and fumaric acid to carry out addition reaction at a temperature of 1 hour; after the addition reaction, add pentaerythritol, gradually heat it to 275°C to carry out the first esterification reaction at a temperature of 6 hours; after the first esterification reaction, cool it to 230°C;
[0099] S3, same as S3 of Example 5;
[0100] S4. Same as S4 in Example 5.
[0101] Comparative Example 3
[0102] A method for preparing a low-odor water-white tackifying resin (nitrogen protection throughout the process):
[0103] S1, preparing refined rosin;
[0104] S2. Accurately weigh linseed oil and refined rosin, grind them and put them into a reaction bottle, heat them to 190°C to melt; add 4,4'-thiobis(6-tert-butyl-3-methylphenol) and acrylic acid to carry out heat-keeping reaction for 1 hour; after the addition reaction is completed, add pentaerythritol, gradually heat up to 275°C to carry out the first esterification reaction for 6 hours; after the first esterification reaction is completed, cool down to 230°C;
[0105] S3, adding glycerol, gradually raising the temperature to 275°C and carrying out the second esterification reaction for 5 hours;
[0106] S4. Same as S4 in Example 6.
[0107] Comparative Example 4
[0108] A method for preparing a low-odor water-white tackifying resin (nitrogen protection throughout the process):
[0109] S1, preparing refined rosin;
[0110] S2. Accurately weigh the refined rosin, crush it, and put it into the reaction bottle, heat it to 190°C to melt it; add 4,4'-thiobis(6-tert-butyl-3-methylphenol) and acrylic acid to carry out heat-insulating addition reaction for 1 hour; after the addition reaction, add pentaerythritol and glycerol, gradually heat it to 275°C to carry out heat-insulating esterification reaction for 8 hours; when the esterification reaction reaches an acid value of <15 mgKOH / g, cool it to 230°C, add linseed oil to carry out heat-insulating modification reaction for 1 hour;
[0111] S3. After the modification reaction is completed, water vapor is introduced for washing for 2 hours, the steam is stopped and vacuum is drawn for 2 hours, the mixture is cooled to 210° C., 2,5-di-tert-butylhydroquinone is added, and the mixture is stirred evenly to obtain the low-odor water-white tackifying resin.
[0112] Test Case
[0113] 1. Softening point: According to GB / T 15332-1994 standard, the ring and ball method is used for determination. The results are shown in Table 2.
[0114] 2. Acid value: Determined according to GB / T 1668-2008 standard method, the results are shown in Table 2;
[0115] 3. Color: measured according to GB / T 3143-1982 standard method, the results are shown in Table 2;
[0116] 4. Aging resistance: Weigh 5 g of each sample (the low-odor water-white tackifying resin of Examples 1-6 and Comparative Examples 1-4), put them into a disposable glass test tube, place them in a 175°C air drying oven for 8 hours, take them out for colorimetry, and measure them according to the iron-cobalt colorimetric method of GB / T 1722-1992. The results are shown in Table 2.
[0117] 5. Volatile matter: Weigh 5 g of each sample (the low-odor water-white tackifying resin of Examples 1-6 and Comparative Examples 1-4) and place them in a small aluminum dish. Then place the sample in a blast drying oven at a constant temperature of 175°C for aging for 4 hours and then take it out. After the sample is cooled to room temperature, accurately weigh it. The weight loss rate is calculated by weighing the mass of the sample after aging, which is the volatile matter. The results are shown in Table 2.
[0118] 6. Odor evaluation:
[0119] (1) Preparation of hot-melt pressure-sensitive adhesive: 49.8 g of the sample (the low-odor water-white tackifying resin of Examples 1-6 and Comparative Examples 1-4) was mixed with 20 g of natural rubber elastomer 1106 (styrene-isoprene-styrene block copolymer, manufactured by Sinopec), 30 g of 4010 cyclohexane oil, 0.1 g of antioxidant 168 and 0.1 g of antioxidant 1010 under molten state to obtain a hot-melt pressure-sensitive adhesive.
[0120] (2) Odor evaluation using hot-melt pressure-sensitive adhesive: 28 g of a sample (a hot-melt pressure-sensitive adhesive prepared using the low-odor water-white tackifying resin of Examples 1-6 and Comparative Examples 1-4) was placed in a glass bottle with a diameter of 60 mm and a height of 90 mm, sealed with tin foil, and heated in a 160°C air drying oven for 3 h. The sample was taken out and cooled to room temperature for sensory odor evaluation. The arithmetic mean of the evaluation grades of all evaluators in the evaluation panel (5 evaluators) was calculated, and the result was retained to one decimal place as the final odor grade of the sample. The odor evaluation grade was 1-5, where 1 was no odor; 2 was slightly odorous; 3 was odorous but acceptable; 4 was strong odorous; and 5 was irritating odor. The results are shown in Table 2.
[0121] Table 2
[0122]
[0123] Result analysis: It can be seen from Table 2 that the water-white tackifying resin obtained in Examples 1-6 of the present invention has good heat resistance, weather resistance and low volatility compared with Comparative Examples 1-4, light color, and low odor for preparing the hot melt pressure-sensitive adhesive, especially Examples 5 and 6 have the best effect.
[0124] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions of the technical solution of the present invention by ordinary technicians in this field do not deviate from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a low-odor water-white tackifying resin, It is characterized in that The following steps are involved: S1, melting rosin and vacuum distilling to obtain refined rosin; S2, heating and melting the refined rosin, adding a catalyst, an unsaturated acid, and a polyol, raising the temperature to carry out a first esterification reaction, cooling after the first esterification reaction, and adding vegetable oil to carry out a modification reaction; S3, after the modification reaction is completed, polyol is added again and the temperature is raised to carry out a second esterification reaction; S4. After the second esterification reaction is completed, washing, dehydration, cooling, and antioxidants are added to obtain the low-odor water-white tackifying resin.
2. The preparation method according to claim 1, It is characterized in that The temperature of the first esterification reaction and the second esterification reaction is 265-285° C., and the time is 4-7 hours.
3. The preparation method according to claim 1, It is characterized in that The temperature of the modification reaction is 220-240° C. and the time is 0.5-1.5 h.
4. The preparation method according to claim 1, It is characterized in that The low-odor water-white tackifying resin comprises the following components in parts by weight: 900-1100 parts of refined rosin, 5-25 parts of vegetable oil, 5-45 parts of unsaturated acid, 70-135 parts of polyol, 2-5 parts of catalyst and 3-10 parts of antioxidant.
5. The preparation method according to claim 4, It is characterized in that The vegetable oil is selected from at least one of tung oil, zelkova oil, castor oil, soybean oil, linseed oil and refined soybean oil.
6. The preparation method according to claim 5, It is characterized in that The vegetable oil is linseed oil and / or soybean oil.
7. The preparation method according to claim 4, It is characterized in that The polyol is selected from at least one of a diol, a triol and a tetraol; the diol is selected from at least one of ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol and neopentyl glycol; the triol is selected from at least one of glycerol, trimethylolethane and trimethylolpropane; the tetraol is selected from at least one of pentaerythritol and dipropylene glycol.
8. A low-odor water-white tackifying resin obtained by the preparation method according to any one of claims 1 to 7.
9. Use of the low-odor water-white tackifying resin obtained by the preparation method according to any one of claims 1 to 7 in the preparation of a pressure-sensitive adhesive.
10. A pressure-sensitive adhesive, It is characterized in that The invention relates to a low-odor water-white tackifying resin obtained by the preparation method according to any one of claims 1 to 7.