Repairable epoxy underfill composition and preparation method thereof

By using specific polypolyols and core-shell toughened particles in the underfill glue to form a nano-scale differential phase island structure, the problem of poor reworkability of the underfill glue in the prior art is solved, and the modulus is reduced at high temperatures is achieved in the high temperature. and adhesion strength improves reworkability and impact resistance, and is suitable for high-reliability chip packaging.

CN118879252APending Publication Date: 2024-11-01COLLTECH DONGGUAN BONDING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410979101.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing underfill glue is difficult to take into account the reworkability, bonding strength and aging resistance, and especially at high temperatures, which shows low reworkability and high adhesiveness, resulting in high packaging defective rate and affecting economic benefits.

Method used

A specific combination of polypolyol and core-shell toughened particles is adopted. The polypolyol does not contain aromatic ring structure, the number average molecular weight is between 2000-3000g/mol, and the hydroxyl value is between 90-120mg KOH/g, forming a nano-scale differential phase island structure. , combined with epoxy resin and silicon micropowder, an island-like structure is formed by thermal curing to absorb curing stress, melting at high temperatures reduces modulus and adhesion strength, and improves reworkability.

Benefits of technology

It achieves the balance of high bonding strength and low CTE at room temperature, while greatly reducing chip shear force at high temperature, providing excellent reworkability and impact resistance, reducing packaging defective yield and improving economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879252A_ABST
    Figure CN118879252A_ABST
Patent Text Reader

Abstract

The invention provides a repairable epoxy underfill composition. The repairable epoxy underfill composition is prepared from the following raw material components in parts by weight: epoxy resin, core-shell toughening particles, a curing agent, polyol and silica powder, the polyhydric alcohol does not contain an aromatic ring structure, the number-average molecular weight of the polyhydric alcohol is 2000-3000 g / mol, and the hydroxyl value of the polyhydric alcohol is 90-120 mg KOH / g. The polyhydric alcohol can form a differential-phase island-shaped structure in epoxy resin after being heated and cured in the presence of the core-shell toughening particles, curing stress can be fully absorbed, the impact resistance of the product in the using process can be improved, and the polyhydric alcohol is crystallized, melted and expanded at high temperature to form micro-droplets; the modulus of the cured glue is sharply reduced, the adhesion strength to a base material is reduced, and the reworkability of the cured glue at a high temperature is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adhesives, and in particular relates to a reworkable epoxy bottom filling composition and a preparation method thereof. Background Art

[0002] The miniaturization and high functionality of electronic devices have increased the requirements for high-density packaging of semiconductor chips and other electronic components. The narrower spacing between large-size high-power chips and the high I / O density have increasingly stringent requirements on the performance of packaging glue. At present, chip packaging is usually directly soldered to the PCB substrate and the difference in the coefficient of thermal expansion (CTE) between the two is large. If the stress caused by the difference in CTE cannot be eliminated, it will cause cracks in the connection part, reducing the connection reliability of the semiconductor chip and the substrate. The bottom composition is used between the chip and the substrate to provide a stronger mechanical connection and reduce the stress on the solder joints caused by the mismatch of the coefficient of thermal expansion between the chip and the substrate. The commonly used bottom composition is mainly composed of a cured epoxy resin filled with a large amount of silica filler. The cured epoxy resin has excellent electrical insulation, high modulus and strength, and good adhesion at different interfaces. It is a good bottom filling glue matrix resin.

[0003] Due to the large size and high price of GPU chips, the bottom filling glue is required to have high processability, reliability and reworkability. When epoxy resin bottom filling glue is used on GPU chips, the glue is usually required to have high moisture and heat resistance, high temperature stability and low CTE. However, this type of glue usually has high Tg performance and high filler filling amount, resulting in high modulus, high temperature and high adhesion, etc., which makes it not reworkable. In commercial mass production, a large number of defective packaging products will be formed due to process problems, which greatly reduces economic benefits. In addition, with the gradual popularization of artificial intelligence, recycling high-cost chips or substrates is conducive to reducing costs and environmental protection, so the industry has a strong demand for bottom filling adhesives with reworkability and high reliability.

[0004] CN118006223A discloses a high-repairability and no-residue bottom filling adhesive and a preparation method thereof. The adhesive comprises the following raw material components by weight: 25-45 parts of bisphenol F epoxy resin, 5-10 parts of trifunctional high-heat-resistant epoxy resin, 5-10 parts of highly flexible polyurethane-modified epoxy resin, 5-15 parts of latent curing agent, 10-25 parts of unsaturated multiolefin acrylic oligomer, 3-10 parts of cross-linked acrylic oligomer, 0.1-1 part of multifunctional acrylic ester oligomer, 5-10 parts of bifunctional acrylic monomer, 0.1-0.8 parts of photoinitiator, 0.5-1 parts of isocyanate cross-linking agent, 0.1-20 parts of spherical silica, and 0.1-5 parts of foamed microspheres. CN117777918A discloses a reworkable toughened chip-level bottom filler and a preparation method thereof, which comprises the following components by weight: 15-25 parts of bisphenol F epoxy resin, 3-8 parts of self-synthesized tetraglycidyl ether containing furan groups, 0.5-2 parts of bismaleimide resin, 0.5-1.5 parts of silane coupling agent, 0.5-1.5 parts of leveling agent, 0.5-1.5 parts of black paste, 60-70 parts of spherical silicon powder, and 5-15 parts of curing agent. Although the CTE of such bottom filler in the prior art is low, the rework performance is still not good enough, and the bonding strength is low. Summary of the invention

[0005] Based on the problem that the bottom filling glue in the above prior art cannot take into account the reworkability, bonding strength and aging resistance, the present invention provides a bottom filling glue and a preparation method thereof, which can ensure good packaging effect while taking into account the reworkability. The present invention solves the above technical problems through the following technical solutions:

[0006] A reworkable epoxy bottom filling composition comprises the following raw material components in parts by weight: epoxy resin, core-shell toughening particles, curing agent, polyol, silicon powder; the polyol does not contain an aromatic ring structure, has a number average molecular weight of 2000-3000 g / mol, and a hydroxyl value of 90-120 mg KOH / g.

[0007] Furthermore, the reworkable epoxy bottom filling composition comprises the following raw material components in parts by weight: 17-25 parts of epoxy resin, 1-5 parts of core-shell toughened particles, 10-20 parts of curing agent, 2-6 parts of polyol, and 55-65 parts of silicon powder.

[0008] Furthermore, the number average molecular weight of the polyol is 2000-2500 g / mol; and the hydroxyl value is 100-110 mg KOH / g.

[0009] Furthermore, after thermal curing, the polyol forms an island structure of nanoscale differential phase in the epoxy resin matrix; further, the size of the nanoscale island structure is 5-500nm, such as 5-200nm, or 5-100nm. The thermal curing temperature is 130-150°C, and the curing time is 0.5-1h.

[0010] The inventors found that the polyol does not have an aromatic ring structure, has highly regular weak polar fragments, and has a specified molecular weight and hydroxyl value. In the bottom filling composition of the present invention, the polyol has a tendency to self-crystallize in the presence of core-shell toughening particles after thermal curing, and will curl up and accumulate by itself, forming an island structure of a nano-scale differential phase in the epoxy resin matrix, which can fully absorb the curing stress, thereby improving the impact resistance of the product during use. At high temperatures (such as 200°C required for rework), crystals melt to form microdroplets, which sharply reduces the modulus of the cured glue and the adhesion strength to the substrate, greatly improving the reworkability of the glue after curing. The differential phase refers to a phase separation structure under microscopic conditions, and the island structure refers to a differential phase structure similar to an island formed in the continuous phase of the polyol in the epoxy resin.

[0011] Furthermore, the core-shell toughening particles are core-shell structure particles with polybutadiene as the shell and polyacrylate as the core, with a size of 200-500nm, and are also dispersed in the glue in the form of microspheres after dispersion. The presence of the core-shell toughening particles in the filling composition does not affect the flow properties of the glue, and the core-shell toughening particles can promote the formation of an island structure of the polyol.

[0012] In a preferred technical solution of the present invention, the core-shell toughened particles are MZ-200 purchased from Kashima Chemical of Japan.

[0013] In the prior art, conventional polyols used in bottom filling glue mainly play a role in increasing flexibility and toughness, and react with acid anhydride, resulting in the polyol being evenly distributed in the epoxy resin to form a homogeneous structure, and being unable to form an island-like differential phase structure. In the bottom filling glue composition of the present invention, the polyol does not react with the acid anhydride, and cooperates with the presence of the core-shell toughening particles to produce a slight differential phase in the glue, promote the self-crystallization of the polyol during the high temperature process, accelerate the phase separation, and form crystalline islands, so that the cured glue has good impact resistance at low temperatures, and at high temperatures, this part of the island crystals will melt to form micro droplets, and the bonding strength will drop significantly, providing excellent high-temperature reworkability. The specific reason is not clear, we believe that the possible reason is that the polyol with a specific structure can be regarded as a surfactant. When the granular core-shell toughening particles are added, the polyol may gather around the core-shell toughening particles to help disperse; at the same time, an aggregation area of ​​the polyol is also formed, and an island-like structured differential phase is formed in the epoxy resin matrix after curing. In order to ensure that the prepared filling composition has a slight differential phase, the polyol should be added as the last step after the accelerator to prevent the components from being dispersed completely evenly, resulting in the polyol being unable to self-crystallize during the thermal curing process, thereby weakening the rework effect at high temperature.

[0014] In a preferred technical solution of the present invention, the polyol is FPS-600 purchased from DIC of Japan, and the core-shell toughened particles are MZ-200 purchased from Kashima Chemical of Japan.

[0015] Furthermore, the epoxy value of the epoxy resin is 0.3-0.7. Specifically, the epoxy resin is selected from at least one of bisphenol epoxy resin and silica-modified epoxy resin; the bisphenol epoxy resin is selected from at least one of bisphenol A epoxy resin, bisphenol F epoxy resin and bisphenol S epoxy resin, preferably a mixture of bisphenol A epoxy resin and bisphenol F epoxy resin, such as ZX-1059; the silica-modified epoxy resin is selected from Nanopox E500.

[0016] Preferably, the epoxy resin is a mixture of bisphenol A epoxy resin and bisphenol F epoxy resin (such as ZX-1059), and a silica-modified epoxy resin in a mass ratio of 4-5:1, such as ZX-1059 and Nanopox E500 in a mass ratio of 12-13:3.

[0017] The curing agent is an acid anhydride curing agent, specifically at least one selected from methylhexahydrophthalic anhydride (MHH-700G), tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, phthalic anhydride, and cyclopentanetetracarboxylic anhydride.

[0018] The silicon micropowder is spherical, with a particle size D50 of 1-2 μm and D100 of 2-6 μm, for example, D50=1.5 μm and D100=3 μm.

[0019] The reworkable epoxy bottom filling composition also includes 1-2 parts by mass of a curing accelerator, 0.2-0.5 parts by mass of a silane coupling agent, and 0.4-1 parts by mass of a nano-color paste. Preferably, the curing accelerator is an imidazole accelerator, such as at least one of 2-ethyl-4-methylimidazole, 2-undecylimidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole; the silane coupling agent is an epoxy silane coupling agent, specifically selected from at least one of A187, KH-561, KH-563, KH-564, A-186, and A-1861; the nano-color paste is a mixture of nano-scale carbon black (10-20nm) and epoxy resin (such as ZX-1059) at a carbon black mass ratio of 30wt%, obtained by three-roll grinding.

[0020] Optionally, the reworkable epoxy underfill composition of the present invention further comprises 0-10 parts of auxiliary agents (e.g., 1-2 parts, 1-5 parts, 3-8 parts), such as thixotropic agents, dispersants, leveling agents, and defoaming agents. The leveling agent is selected from at least one of BYK-354, BYK-310, levelol 495, MOK-2024, TEGO 450, KYC-616, FLOW-200, and FLOW-450; the dispersant is selected from at least one of BYK-9010, BYK-995, BYK-306, BYK-2008, and BYK-2009; the defoaming agent is selected from at least one of BYK-320, BYK-322, and BYK-323; and the thixotropic agent is fumed silica.

[0021] The epoxy resin and curing agent ensure the viscosity, reactivity, bonding strength and heat resistance of the bottom filling glue. The addition of silicon micropowder filler improves the thermal expansion coefficient and modulus of the bottom filling glue. The bottom filling glue is adjusted by adding the additives to improve the dispersibility of the filler in the resin matrix and the bonding force between the resin and the filler. At the same time, the wettability of the bottom filling glue to the substrate is also improved, so that the degree of grease overflow is controlled, and the bottom filling glue obtained has suitable viscosity and good fluidity.

[0022] The core of the technical solution of the present invention lies in the selection and combination of core-shell toughened particles, polyols and epoxy resins. The reworkable high-reliability epoxy bottom filling composition of the present invention has excellent toughness, and provides good chip shear force at room temperature or device operating temperature while taking into account moisture and heat resistance, high Tg and low CTE. However, the chip shear force drops significantly at high temperatures, for example, it can drop to below 1.5 MPa at 200°C, preferably below 1 MPa. The preferred embodiment of the present invention can even reach 0 MPa, providing very excellent reworkability.

[0023] The reworkable high-reliability epoxy underfill composition of the present invention has a high storage modulus at room temperature after being fully cured, for example, greater than 3.5 GPa at 25°C, including greater than 4.0 GPa or greater than 5.0 GPa, thereby providing good bonding strength at room temperature or device use temperature, but the storage modulus drops significantly at high temperature, for example, it can drop to below 210 MPa at 200°C, including below 150 MPa or 100 MPa, providing the possibility of high-temperature rework. The storage modulus is obtained based on DMA testing.

[0024] After being completely cured, the reworkable high-reliability epoxy underfill composition of the present invention has a glass transition temperature (Tg) of not less than 100° C., preferably a glass transition temperature of 110-120° C. The glass transition temperature is measured by DSC.

[0025] The present invention also provides a method for preparing the above-mentioned reworkable epoxy underfill composition, comprising the following steps:

[0026] Except for the polyol, all other raw materials are added into a dual planetary power mixing device, vacuumed, stirred and mixed evenly, and finally the polyol is added, stirred and mixed evenly to obtain a reworkable epoxy bottom filling composition.

[0027] Furthermore, the preparation method of the reworkable epoxy underfill composition comprises the following steps:

[0028] (S1) adding epoxy resin, toughened core-shell particles, and optionally adding additives, and stirring evenly;

[0029] (S2) After heating to 50-70°C, add silicon micropowder and stir evenly;

[0030] (S3) cooling to room temperature, adding a curing agent and stirring evenly;

[0031] (S4) adding polyol, stirring evenly and performing vacuum degassing to obtain a reworkable epoxy bottom filling composition.

[0032] Preferably, the stirring device is a dual planetary power mixing device.

[0033] Furthermore, the method for preparing the reworkable epoxy underfill composition comprises the following steps:

[0034] (S1) adding epoxy resin, toughened core-shell particles, silane coupling agent, and optionally, auxiliary agent, and stirring evenly;

[0035] (S2) After heating to 50-70°C, add silicon micropowder and stir evenly;

[0036] (S3) cooling to room temperature, adding curing agent, curing accelerator and nano color paste and stirring evenly;

[0037] (S4) adding polyol, stirring evenly and performing vacuum degassing to obtain a reworkable epoxy bottom filling composition.

[0038] The purpose of adding the polyol after the accelerator is to prevent the components from being dispersed completely evenly, so that the polyol forms the required island structure in the epoxy resin and improves the reworkability.

[0039] Compared with the prior art, the present invention has achieved the following beneficial effects:

[0040] 1. The present invention uses a specific polyol in the bottom filling composition based on epoxy resin, which does not contain an aromatic ring structure, has a number average molecular weight of 2000-3000g / mol, and a hydroxyl value of 90-120mg KOH / g, preferably a polyol with a number average molecular weight of 2000-2500g / mol and a hydroxyl value of 100-110mg KOH / g. The polyol has a tendency to self-crystallize and does not react with an anhydride curing agent. In the presence of core-shell toughening particles, a nano-scale differential phase structure, i.e., an island structure, is formed in the epoxy resin after thermal curing, which can fully absorb the curing stress, thereby improving the impact resistance of the product during use; and at high temperature (such as 200°C), the crystallization melt expands to form micro droplets, which sharply reduces the modulus of the cured glue and reduces the adhesion strength to the substrate, greatly improving the repairability of the cured glue. The repairability is good.

[0041] 2. The present invention combines the good filling properties, low CTE, and high Tg of the bottom filling glue by combining and adding various raw materials in a reasonable ratio and optimizing the preparation process. It can be used as a high-reliability bottom filling glue suitable for automotive chips and high-performance large chips.

[0042] 3. The bottom filling composition of the present invention can also be used to adjust the use of other additives, such as fumed silica, to prepare a high-viscosity, high-thixotropic glue with the above-mentioned advantages for chip corner bonding, coating and dam, making the product more widely applicable. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a SEM image of the bottom filling glue of Example 1 after curing.

[0044] Figure 2 This is the SEM image of the bottom filling glue after curing in comparative example 1.

[0045] Figure 3 This is the SEM image of the bottom filling glue after curing in comparative example 2.

[0046] Figure 4 This is the SEM image of the bottom filling glue after curing in comparative example 3. DETAILED DESCRIPTION

[0047] The present invention is further described below in conjunction with specific examples, but the present invention is not limited to the following examples. The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified. A specific example is given below to help understand the dual inorganic composite solid electrolyte described in the present invention.

[0048] The hydroxyl value of polyol FPS-600 is 102.2 mg KOH / g, and the number average molecular weight is about 2000 g / mol.

[0049] Silica powder D50=1.5μm, D100=3μm.

[0050] The nano color paste is obtained by mixing nano carbon black (20nm) and epoxy resin (ZX-1059) in a mass ratio of 3:7 and grinding by three rollers.

[0051] Example 1

[0052] The components of the epoxy underfill composition of this embodiment are as follows in parts by mass:

[0053] Epoxy resin ZX-1059 12.1

[0054] Epoxy Resin Nanopox E500 3

[0055] Core-shell toughened particles MZ-200 4

[0056] Dispersant BYK-W9010 0.3

[0057] Silane coupling agent A187 0.2

[0058] Polyol FPS-600 3

[0059] Silica powder 60

[0060] Anhydride curing agent MHH-700G 16

[0061] Curing accelerator 1

[0062] Nano color paste 0.4

[0063] The curing accelerator is prepared by adding 25 parts of 2MZ-A and 25 parts of 2PHZ-PW into a stirring tank and stirring in a homogenizer. The temperature is controlled to be less than 35°C. After stirring evenly, the mixture is passed through a ceramic three-roller for three times. The roller spacing is controlled to be 100 / 50μm, 50 / 25μm, and 10 / 5μm respectively. After three rollers, the mixture is stirred and dispersed in a homogenizer again to obtain an accelerator mixture, which is then stored in a -20°C refrigerator.

[0064] Preparation process of epoxy bottom filling composition: clean dual planetary power mixing equipment, add ZX-1059, Nanopox E500, core-shell toughened particles MZ-200, BYK-W9010, A187 and stir well, set the temperature of the reactor to 65±5°C, add silicon powder three times, stir evenly, control the indoor humidity to <45%, set the roller temperature of the three-roller machine to 45°C, the roller spacing to 20 / 10um, mix the materials after three rollers, put them into the reactor for dehydration, stirring and dispersion, add MHH-700G, curing accelerator, nano color paste after cooling to room temperature, stir evenly and vacuum degas, finally add polyol FPS-600, stir evenly and vacuum degas, obtain the bottom filling composition, and package and refrigerate in time.

[0065] Comparative Example 1

[0066] Other conditions and operations were the same as those in Example 1, except that the polyol FPS-600 was replaced by an equal amount of polypropylene glycol with a number average molecular weight of 2000 and a hydroxyl value of 126 mgKOH / g.

[0067] Comparative Example 2

[0068] Other conditions and operations were the same as those in Example 1, except that the core-shell toughened particles were replaced by an equal mass of Arkema toughened resin XT-100 (non-core-shell structure, MMA and polyurethane block polymer) instead of MZ-200.

[0069] Comparative Example 3

[0070] Other conditions and operations were the same as those in Example 1, except that the polyol FPS-600 was replaced by an equal mass of polyethylene terephthalate (number average molecular weight of about 2000 g / mol).

[0071] Figure 1 This is a SEM image of the bottom filling glue after curing in Example 1. It can be seen that there is an obvious differential phase island structure in the epoxy resin, and the size of the island structure is 5-200nm.

[0072] Figure 2 , Figure 3 , Figure 4They are SEM images of comparative examples 1-3 after the glue is cured. It can be seen that the polyol is replaced by a conventional polyol, and the hydroxyl value does not meet the requirements (comparative example 1, Figure 2 ), or the core-shell toughening particles are replaced with conventional non-core-shell toughening resins (Comparative Example 2, Figure 3 ); The polyol contains an aromatic ring structure (Comparative Example 3, Figure 4 ) cannot effectively form an island structure, so the reworkability at high temperature is significantly reduced.

[0073] Example 2

[0074] The components of the epoxy underfill composition of this embodiment are as follows in parts by mass:

[0075] Epoxy resin ZX-1059 12.1

[0076] Epoxy Resin Nanopox E500 3

[0077] Core-shell toughened particles MZ-200 4

[0078] Dispersant BYK-W9010 0.3

[0079] Silane coupling agent A187 0.2

[0080] Polyol FPS-600 6

[0081] Silica powder 60

[0082] Anhydride curing agent MHH-700G 16

[0083] Curing accelerator 1

[0084] Nano color paste 0.4

[0085] The composition of the curing accelerator is: a mixture of 25 parts of imidazole 2MZ-A and 25 parts of imidazole 2PHZ-PW. The preparation process is to add 25 parts of 2MZ-A and 25 parts of 2PHZ-PW into a stirring tank and stir in a homogenizer, control the temperature to be less than 35°C, and after stirring evenly, pass through a ceramic three-roller for three times, and the roller spacing is controlled to be 100 / 50um, 50 / 25um, and 10 / 5um respectively. After three rollers, the accelerator mixture is stirred and dispersed in a homogenizer again, and stored in a -20°C refrigerator.

[0086] Preparation process of bottom filling glue: thoroughly clean the dual planetary power mixing equipment, add ZX-1059, NanopoxE500, core-shell toughening resin MZ-200, BYK-W9010, and A187 respectively, stir well, set the temperature of the reactor to 65±5℃, add silicon powder in 3 batches, stir evenly, control the indoor humidity to <45%, set the roller temperature of the three-roll machine to 45℃, and the roller spacing to 20 / 10um. After the three rollers, the mixed material is re-weighed and put into the reactor for dehydration, stirring and dispersion. After cooling, add MHH-700G, nano color paste, and curing accelerator mixture, stir evenly again and vacuum degas, and finally add polyol FPS-600 and stir evenly to obtain the bottom filling composition.

[0087] Example 3

[0088] The composition of the product in Example 3 is as follows by weight. Compared with Example 1, the difference is that fumed silica TS-720 is added to adjust the viscosity and thixotropy.

[0089] Epoxy resin ZX-1059 12.1

[0090] Epoxy Resin Nanopox E500 3

[0091] Core-shell toughened particles MZ-200 4

[0092] Dispersant BYK-W9010 0.1

[0093] Silane coupling agent A187 0.2

[0094] Polyol FPS-600 3

[0095] Silica powder 58.5

[0096] Anhydride curing agent MHH-700G 16

[0097] Accelerator 1

[0098] Fumed Silica TS-720 1.5

[0099] Nano color paste 0.4

[0100] Compared with Example 1, this embodiment adds a fumed silica thixotropic agent to obtain a bottom filling adhesive with high thixotropic properties, making the product more widely applicable.

[0101] Preparation process of epoxy bottom filling composition: clean dual planetary power mixing equipment, add ZX-1059, Nanopox E500, core-shell toughened particles MZ-200, BYK-W9010, A187, TS-720 and stir well, set the temperature of the reactor to 65±5°C, add silicon powder three times, stir evenly, control the indoor humidity to <45%, set the roller temperature of the three-roller machine to 45°C, the roller spacing to 20 / 10um, mix the materials after three rollers, put them into the reactor for dehydration, stirring and dispersion, add MHH-700G, curing accelerator, nano color paste after cooling to room temperature, stir evenly and vacuum degas, finally add polyol FPS-600, stir evenly and vacuum degas, obtain the bottom filling composition, and package and refrigerate in time.

[0102] Example 4

[0103] The other conditions were the same as those in Example 1, except that the epoxy resin was changed from a compound of 12.1 parts by mass of ZX-1059 and 3 parts by mass of Nanopox E500 to 15.1 parts by mass of ZX-1059.

[0104] Example 5

[0105] The other conditions were the same as those in Example 1, except that the epoxy resin was changed from a compound of 12.1 parts by mass of ZX-1059 and 3 parts by mass of Nanopox E500 to 15.1 parts by mass of Nanopox E500.

[0106] Application Examples

[0107] The bottom filling glue of the above-mentioned embodiment and comparative example was subjected to the following performance test, and the curing condition was 150℃ / 30min. The results are shown in Table 1 below. Among them, CTEα1 represents the thermal expansion coefficient below Tg, and CTEα2 represents the thermal expansion coefficient above Tg. Reworkability can be characterized by chip shear strength. After the reworkable high-reliability epoxy bottom filling composition of the present invention is fully cured, the chip shear strength at room temperature is greater than 20MPa, but the chip shear strength will drop significantly at high temperature. For example, at 200℃, the chip shear strength is less than 2.5MPa, or even less than 1.0MPa. The chip shear strength is tested based on the flat push method of a 2×2mm single crystal silicon chip on a PCB. The anti-drop experiment is to perform a drop test on 20 chips at a height of 1m. 0 / 20 means that 0 of the 20 test chips failed the test, and the rest are analogous to this meaning.

[0108] Table 1 Bottom filling glue performance test

[0109]

[0110]

Claims

1. A reworkable epoxy underfill composition, characterized in that: The invention comprises the following raw material components in parts by weight: epoxy resin, core-shell toughening particles, curing agent, polyol and silicon powder; the polyol does not contain aromatic ring structure, has a number average molecular weight of 2000-3000 g / mol and a hydroxyl value of 90-120 mg KOH / g.

2. The reworkable epoxy underfill composition according to claim 1, characterized in that: The polyol does not contain an aromatic ring structure, has a number average molecular weight of 2000-2500 g / mol, and a hydroxyl value of 100-110 mg KOH / g.

3. The reworkable epoxy underfill composition according to claim 1, characterized in that: The polyol can form an island structure of a differential phase in the epoxy resin after being heated and solidified in the presence of core-shell toughening particles; preferably, the island structure refers to a differential phase structure with a size of 5-500 nm formed by the polyol in the epoxy resin continuous phase.

4. The reworkable epoxy underfill composition according to claim 1, characterized in that: The core-shell toughening particles are core-shell structure particles with polybutadiene as the shell and polyacrylate as the core, and the size is 200-500nm.

5. The reworkable epoxy underfill composition according to claim 1, characterized in that: The polyol is FPS-600 purchased from DIC of Japan, and the core-shell toughened particles are MZ-200 purchased from Kashima Chemical of Japan.

6. The reworkable epoxy underfill composition according to claim 1, characterized in that: The epoxy value of the epoxy resin is 0.3-0.7; the epoxy resin is selected from at least one of bisphenol epoxy resin and silica-modified epoxy resin, and the bisphenol epoxy resin is selected from at least one of bisphenol A epoxy resin, bisphenol F epoxy resin and bisphenol S epoxy resin, preferably a mixture of bisphenol A epoxy resin and bisphenol F epoxy resin.

7. The reworkable epoxy underfill composition according to claim 6, characterized in that: The epoxy resin is a compound of ZX-1059 and Nanopox E500 in a mass ratio of 12-15:

3.

8. The reworkable epoxy underfill composition according to claim 1, characterized in that: The invention comprises the following raw material components in parts by weight: 17-25 parts of epoxy resin, 1-5 parts of core-shell toughening particles, 10-20 parts of curing agent, 2-6 parts of polyol and 55-65 parts of silicon micropowder.

9. The reworkable epoxy underfill composition according to claim 1, characterized in that: The curing agent is an acid anhydride curing agent; preferably at least one of methylhexahydrophthalic anhydride (MHH-700G), tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, phthalic anhydride, and cyclopentanetetracarboxylic anhydride.

10. The reworkable epoxy underfill composition according to claim 1, characterized in that: The reworkable epoxy underfill composition further includes a curing accelerator and a silane coupling agent.

11. The reworkable epoxy underfill composition according to claim 10, characterized in that: The curing accelerator is selected from imidazole curing accelerators; preferably at least one of 2-ethyl-4-methylimidazole, 2-undecylimidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole; the epoxy silane coupling agent ring is selected from at least one of A187, KH-561, KH-563, KH-564, A-186, and A-1861.

12. The reworkable epoxy underfill composition according to claim 1, characterized in that: The silicon micropowder is spherical, with a particle size D50 of 1-3 μm and a particle size D100 of 2-10 μm.

13. The reworkable epoxy underfill composition according to claim 1, characterized in that: After the filling composition is completely cured, its glass transition temperature is greater than 110° C., the room temperature chip shear force is greater than 25 MPa, and the 200° C. chip shear force is less than 1.5 MPa.

14. The method for preparing the reworkable epoxy underfill composition according to any one of claims 1 to 13, characterized in that: The following steps are involved: All raw materials except the polyol are added into a stirring device, vacuumed, stirred and mixed evenly, and finally the polyol is added, stirred and mixed evenly to obtain a reworkable epoxy bottom filling composition.

15. The preparation method according to claim 14, characterized in that: The following steps are involved: (S1) adding epoxy resin, toughened core-shell particles, and optionally adding additives, and stirring evenly; (S2) After heating to 50-70°C, add silicon micropowder and stir evenly; (S3) cooling to room temperature, adding a curing agent and stirring evenly; (S4) adding polyol, stirring evenly and performing vacuum degassing to obtain a reworkable epoxy bottom filling composition.

16. The preparation method according to claim 14, characterized in that: The following steps are involved: (S1) adding epoxy resin, toughened core-shell particles, silane coupling agent, and optionally, auxiliary agent, and stirring evenly; (S2) After heating to 50-70°C, add silicon micropowder and stir evenly; (S3) cooling to room temperature, adding curing agent, curing accelerator and nano color paste and stirring evenly; (S4) adding polyol, stirring evenly and performing vacuum degassing to obtain a reworkable epoxy bottom filling composition.