Preparation method and application of polyvinyl alcohol-based dual-network aerogel shaped composite phase change energy storage material
By using organic and inorganic composite phase change materials packaged by polyvinyl alcohol-based dual-network aerogel in building thermal management, the problems of liquid leakage, supercooling and flammability are solved, and the enthalpy of phase change and mechanical strength are improved, achieving excellent results building thermal management performance.
Patent Information
- Application Number
- CN202410911820.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-01
AI Technical Summary
In the field of building thermal management, existing phase change materials have problems such as liquid leakage, supercooling, phase separation and flammability, and the packaging materials have low porosity and insufficient strength, resulting in low phase change enthalpy and mechanical strength, which makes it difficult to be effective. Reduce building energy consumption.
Polyvinyl alcohol-based double network aerogel encapsulates organic inorganic composite phase change materials, and a stable double network structure is formed by introducing a second inorganic nanomaterial, which increases flame retardant performance and mechanical strength, and adds nucleating agent to reduce supercooling , an organic inorganic composite phase change material with high phase change enthalpy and good cycle stability is formed.
It achieves excellent flame retardant performance, low supercooling and phaseless separation problems, improves phase change enthalpy value and mechanical strength, significantly improves building thermal management performance, and is suitable for large-scale applications.
Smart Images

Figure CN118879281A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of a polyvinyl alcohol-based double-network aerogel-shaped organic-inorganic composite phase-change energy storage material, and belongs to the technical field of phase-change energy storage. Background Art
[0002] With the continuous growth of global energy demand, building energy consumption has become an urgent problem to be solved worldwide. According to statistics, the construction industry consumes about 30% of the world's energy, which not only increases the pressure on energy supply, but also aggravates the risk of environmental pollution and climate change. Therefore, it is urgent to find effective energy-saving solutions to reduce building energy consumption and improve energy efficiency. Among the many energy-saving technologies, thermal energy storage technology has attracted much attention because of its ability to effectively regulate and manage thermal energy. Thermal energy storage technology stores excess thermal energy when needed and releases it when needed, so that buildings can maintain a more stable internal environment during temperature fluctuations, thereby reducing the frequency of use of air conditioning and heating equipment and achieving energy-saving effects.
[0003] Among various thermal energy storage technologies, phase change materials have shown significant application advantages due to their unique characteristics of absorbing and releasing a large amount of heat during the phase change process. Therefore, studying the application of phase change materials in buildings and developing efficient phase change material composite structures have become one of the important directions for reducing building energy consumption. Among various types of PCMs, solid-liquid phase change materials have attracted extensive attention from researchers due to their small volume change and sensitive temperature response. Solid-liquid phase change materials can be divided into organic, inorganic and organic-inorganic composite phase change materials according to their composition structure. Organic phase change materials have the advantages of non-corrosiveness, low supercooling, good thermal stability and chemical stability, but also have the disadvantages of flammability and low thermal conductivity; inorganic phase change materials have the advantages of high thermal conductivity and high phase change enthalpy, but have the problems of high supercooling and easy phase separation. Organic-inorganic composite phase change materials have become a research hotspot in recent years because they have the advantages of both organic and inorganic phase change materials. However, the application of composite phase change materials in the field of building thermal management still faces two major challenges: first, the liquid generated during the phase change process is prone to leakage. Secondly, the low phase change enthalpy leads to poor utilization effect. In recent years, aerogel has been considered as an ideal supporting material to solve the problem of PCM leakage due to its ultra-high porosity and specific surface area, and because of the ultra-high loading rate of aerogel, the phase change material can also maintain a high phase change enthalpy. This is because the phase change material can achieve efficient adsorption in aerogel, thereby obtaining an ultra-high energy storage density. Many researchers have combined aerogel with phase change materials and applied them to many fields such as infrared stealth, seawater desalination, and solar thermal energy capture and storage.
[0004] At present, many researchers have applied phase change materials to building thermal management. However, these studies still have some problems that have not been completely solved, such as supercooling, phase separation or flammability. Although some researchers have tried to solve these problems by adding flame retardants, nucleating agents and thickeners, this will undoubtedly significantly reduce the phase change enthalpy of composite phase change materials. In addition, most phase change materials used in the construction field are usually encapsulated with porous materials such as diatomaceous earth, perlite and kaolinite to prevent leakage. However, these encapsulation materials have the defects of low porosity and insufficient strength, resulting in low phase change enthalpy and mechanical strength of the prepared composite phase change materials, which in turn reduces its effectiveness in building thermal management. Summary of the invention
[0005] To address the above problems, we first compounded high enthalpy organic phase change materials and inorganic phase change materials to form organic-inorganic composite phase change materials, and then added nucleating agents to solve the supercooling problem of organic-inorganic phase change materials. Secondly, we introduced a second inorganic nanomaterial into the polyvinyl alcohol matrix, which cross-linked with polyvinyl alcohol through supramolecular forces to form a stable double-network structure aerogel for encapsulating organic-inorganic composite phase change materials. Finally, we used the prepared polyvinyl alcohol-based double-network aerogel to encapsulate organic-inorganic composite phase change materials, successfully prepared a double-network aerogel-based organic-inorganic composite phase change material, and applied it to building thermal management.
[0006] Based on the flame retardancy of inorganic phase change materials, low supercooling and no phase separation of organic phase change materials, this work uses nucleating agents to reduce the supercooling of the system, and constructs an organic-inorganic composite phase change material system with excellent flame retardancy, low supercooling and no phase separation problem; due to the poor thermal stability, insufficient mechanical strength and flammability of polyvinyl alcohol aerogel, it is difficult to apply it in the field of construction. We introduced a second inorganic nanomaterial into the polyvinyl alcohol aerogel matrix, which cross-linked with polyvinyl alcohol through supramolecular forces to form a stable double network structure to increase the flame retardancy and mechanical strength of polyvinyl alcohol. An aerogel-based composite phase change material with good shape stability and high mechanical strength was constructed. The research results show that the prepared CPCM has a high phase change enthalpy value and good cyclic stability. In addition, the CPCM also shows excellent building thermal management performance, which is very suitable for large-scale application in building thermal management in the future.
[0007] The invention discloses a preparation method and application of a polyvinyl alcohol-based double network aerogel-shaped organic / inorganic composite phase change energy storage material, wherein the polyvinyl alcohol-based double network aerogel-shaped organic / inorganic phase change energy storage material is composed of 30-70wt% of inorganic solid-liquid phase change material, 40-60wt% of organic solid-liquid phase change material, 0.1-5wt% of nucleating agent and 5-20wt% of porous supporting material by mass percentage. The inorganic solid-liquid phase change material is a hydrated inorganic salt phase change material, the organic solid-liquid phase change material is an organic nitride, an organic acid ester or a long-chain alkane phase change material, the nucleating agent is a nano-oxide or a salt with a similar crystal form, and the porous supporting material is a second inorganic nano-material introduced into the polyvinyl alcohol matrix, which is cross-linked with the polyvinyl alcohol through supramolecular forces to form a stable double network structure for increasing the flame retardancy and mechanical strength of the polyvinyl alcohol.
[0008] Preferably, the organic / inorganic composite solid-liquid phase change material is composed of 40-50wt% inorganic solid-liquid phase change material, 45.5wt% organic solid-liquid phase change material, 1.0wt% nucleating agent and 5-20wt% porous support material by mass percentage. The phase change material can maintain a uniform and stable shape with low supercooling, meeting the thermal management requirements.
[0009] More preferably, the organic-inorganic composite solid-liquid phase change material consists of 45.5wt% of inorganic solid-liquid phase change material, 45.5wt% of organic solid-liquid phase change material, 1.0wt% of nucleating agent and 8.0wt% of porous supporting material in percentage by mass.
[0010] Preferably, the inorganic solid-liquid phase change material is one to three of sodium acetate trihydrate, calcium sulfate dihydrate, potassium aluminum sulfate dodecahydrate, ammonium aluminum sulfate dodecahydrate, magnesium chloride hexahydrate, magnesium sulfate heptahydrate, calcium nitrate tetrahydrate, zinc chloride hexahydrate and sodium thiosulfate pentahydrate.
[0011] Preferably, the organic solid-liquid phase change material is one to three of urea, erythritol, xylitol, mannitol, erythritol, polyethylene glycol, neopentyl glycol, capric acid, lauric acid, palmitic acid and stearic acid.
[0012] Preferably, the nucleating agent is one to three of titanium dioxide, aluminum oxide, zinc oxide, sodium chloride, nanosilver, nanocopper, nanogold, disodium hydrogen phosphate, sodium silicate nonahydrate, silicon dioxide, disodium hydrogen phosphate dodecahydrate, and sodium metasilicate nonahydrate.
[0013] Preferably, we add some ionic cellulose gum such as xanthan gum, polysorbate or sodium carboxymethyl cellulose as a thickener to the organic-inorganic composite phase change material to solve the phase separation problem of the organic-inorganic phase change material.
[0014] Preferably, the porous supporting material body is polyvinyl alcohol aerogel.
[0015] More preferably, the porous support material polyvinyl alcohol aerogel as a new material has the advantages of low density and high porosity, but also has the following disadvantages:
[0016] 1. Poor thermal stability, easy to decompose and lose its mechanical strength in high temperature environment.
[0017] 2. The mechanical strength is limited and it is easy to break under mechanical impact or stretching.
[0018] 3. Flammable. Polyvinyl alcohol itself is a combustible material and is easy to burn under high temperature and open flame environment. Therefore, it is not suitable for applications with high fire protection requirements, such as the construction field.
[0019] Therefore, we introduced 1 to 3 inorganic nanomaterials including silica, alumina, titanium dioxide, zirconium dioxide, montmorillonite, carbon nanotubes, nanosilicate, nickel foam, aluminum foam, copper foam, kaolin and mesoporous carbon into polyvinyl alcohol aerogel to form a double network structure to increase the flame retardant properties and mechanical strength of polyvinyl alcohol.
[0020] More preferably, in view of the above problems, we cross-link hydrophilic silica and polyvinyl alcohol to prepare double network aerogel to solve the above problems. There are a large number of hydroxyl groups on the molecular chain of polyvinyl alcohol, which interact with the silanol groups on the surface of silica through hydrogen bonds to form a stable three-dimensional network structure. This network structure can enhance the mechanical strength and stability of the aerogel. At the same time, due to the excellent flame retardant properties and thermal stability of silica, the thermal stability and flame retardant properties of the cross-linked double network aerogel are greatly improved.
[0021] More preferably, the inorganic solid-liquid phase change material is sodium acetate trihydrate, the organic solid-liquid phase change material is urea, the nucleating agent is disodium hydrogen phosphate dodecahydrate, and the porous supporting material is polyvinyl alcohol-based double-network aerogel.
[0022] More preferably, the organic / inorganic composite phase change material is composed, by mass percentage, of 45.5wt% of urea as an organic phase change material, 45.5wt% of sodium acetate trihydrate as an inorganic phase change material, 1.0wt% of disodium hydrogen phosphate dodecahydrate as a nucleating agent, and 8.0wt% of polyvinyl alcohol-based double-network aerogel as a porous support material.
[0023] Another object of the present invention is to provide a method for preparing the above-mentioned organic / inorganic composite phase change material suitable for building thermal management.
[0024] A method for preparing a polyvinyl alcohol-based double-network aerogel-shaped organic / inorganic composite phase-change energy storage material with a heat-insulating function, comprising the following process steps:
[0025] (1) firstly heat and melt the inorganic hydrated salt phase change material in a water bath, and then stir to obtain a hydrated salt solution for use;
[0026] (2) dissolving and mixing the organic phase change material and the inorganic hydrated salt solution under heating conditions in a water bath to form an organic-inorganic composite phase change material. Then, adding an appropriate amount of nucleating agent to reduce the supercooling problem of the composite phase change material, stirring evenly to obtain an organic / inorganic composite phase change material;
[0027] (3) Dissolve the polyvinyl alcohol powder in deionized water for half an hour, stir for 30 minutes, add the inorganic nanomaterial and mix well, then pour the solution into a mold. After freezing the mold in a -20°C refrigerator for 12 hours, put it in a freeze dryer and dry it for 24 hours to obtain the polyvinyl alcohol-based double network aerogel.
[0028] (4) Preparing a shaped organic / inorganic composite phase change material by vacuum impregnation: melting the above organic / inorganic composite phase change material; adding polyvinyl alcohol-based double network aerogel thereto for encapsulation; and vacuum impregnating for 2 hours to obtain a shaped organic / inorganic composite phase change material.
[0029] Furthermore, the specific steps are:
[0030] Step 1: Preparation of organic / inorganic composite materials:
[0031] First, 4g urea and 6g sodium acetate trihydrate were mixed and placed in a 20mL transparent glass bottle, and the total mass of the mixture was controlled to be 10g. Secondly, it was placed in a 70℃ water bath to dissolve for 120min and then set aside. Finally, it was placed under magnetic stirring for 30min and then set aside. Then, 0.1g disodium hydrogen phosphate dodecahydrate was added to solve the supercooling problem of the composite system, and the mixture was stirred for 30 minutes under magnetic stirring to obtain an organic-inorganic composite phase change material.
[0032] Step 2: Preparation of polyvinyl alcohol-based double network aerogel:
[0033] The preparation method of polyvinyl alcohol-based double network aerogel is as follows: dissolve 2.0g of polyvinyl alcohol powder in deionized water at 85°C for half an hour, stir for 30 minutes, and then pour the solution into a mold. After the mold is frozen in a -20°C refrigerator for 12 hours, it is placed in a freeze dryer and dried for 24 hours to obtain polyvinyl alcohol aerogel. The preparation method of polyvinyl alcohol-silica (PVA-SiO2) aerogel is similar to that of polyvinyl alcohol aerogel, except that after the polyvinyl alcohol powder is completely dissolved, 1.5g of silica is added and stirred for half an hour, and other conditions are the same. The preparation of PVA / SiO2 / CNTs aerogel is based on PVA / SiO2 aerogel, and an additional 15g of carbon nanotube dispersion is added, and the other conditions remain unchanged.
[0034] Step 3: Preparation of shaped phase change material:
[0035] The shaped organic / inorganic composite phase change material was prepared by vacuum impregnation method. The preparation method is as follows: first, the prepared organic / inorganic composite phase change material is placed in a 100mL beaker, and then placed in a vacuum drying oven at 60°C to melt for standby use. Secondly, polyvinyl alcohol-based double network aerogel is added thereto, and the shaped organic / inorganic composite phase change material is obtained by placing it in a vacuum drying oven for vacuum adsorption for 2 hours.
[0036] Preferably, the phase change temperature point of the phase change material used for building thermal management should be within 19-40°C.
[0037] More preferably, the phase change temperature of the organic-inorganic composite phase change material is 29.4°C.
[0038] More preferably, the phase change temperature of the fixed organic-inorganic composite phase change material is 28.3°C.
[0039] More preferably, the phase change enthalpy of the shaped organic-inorganic composite phase change material is 194.3 J / g.
[0040] Another object of the present invention is that the organic / inorganic composite phase change material can be applied to the field of building energy conservation. Building energy consumption accounts for one-third of the world's energy consumption, so it is necessary to conduct building thermal management to save energy. Studies have shown that adding an appropriate amount of phase change materials to buildings can significantly improve indoor comfort conditions and reduce the energy demand of HVAC systems. Specifically, in the field of building thermal management, phase change materials are directly integrated into building structures for thermal management, and the thermal mass and thermal inertia of lightweight buildings are improved by utilizing the latent heat capacity of phase change materials. Phase change materials in buildings can absorb solar energy and convert it into heat and store it in the form of latent heat, while reducing external heat diffusion during hot periods during the day. The stored heat is released during non-peak hours (nighttime) to maintain the room temperature at a certain level or reduce the amplitude of indoor temperature fluctuations.
[0041] The beneficial effects of the present invention are:
[0042] In order to evaluate the test effect of the prepared phase change aerogel composite material in hot outdoor, we chose to conduct actual application tests on it. We built a simple building model to test the application effect of a polyvinyl alcohol-based double network aerogel-shaped organic / inorganic composite phase change energy storage material with thermal insulation function. As shown in the figure, we filled the foam and CPCM into the interlayer and the top respectively, tested them under outdoor sunlight to increase the internal temperature of the model, and tested the time required for heating. Then move it to a 0℃ constant temperature and humidity chamber to cool it down (simulating the low temperature outdoor at night), and test the time required for cooling.
[0043] Judging from the results, the indoor temperature rise rate of the foam group is much faster than that of the experimental group. This is because the fixed organic-inorganic composite phase change material must first undergo a phase change heat storage process under solar radiation, and then transfer heat to the room, thereby maintaining the indoor temperature at a relatively low state for a certain period of time. The rapid increase in indoor temperature in the foam group is due to direct radiation from sunlight. When both groups of models were moved to a constant temperature and humidity chamber at 0°C, the indoor temperature of the foam group dropped instantly, while the temperature of the CPCM group changed slowly. The CPCM group maintained the indoor temperature above 18°C for 8.7 times longer than the blank group, which shows that the composite phase change material has phase change heat release in this process, maintaining the room temperature relatively stable, reducing the fluctuation range of indoor air temperature, and increasing body surface comfort. In summary, CPCM can significantly delay the heating and cooling time inside the building, has good building thermal management capabilities, and has great practical application value.
[0044] The present invention discloses a high enthalpy organic / inorganic composite phase change material suitable for thermal management of building outer insulation. We selected SAT with a phase change temperature of 57.5°C and a phase change enthalpy of 257.6 J / g as the main phase change material, but its phase change temperature is still higher than the ideal building required temperature. Therefore, we use composite means to adjust the phase change temperature point of SAT. Finally, we selected UREA to form a composite mixture with SAT to reduce the phase change temperature point of SAT to meet the application requirements of building thermal management.
[0045] In order to determine the optimal ratio of UREA / SAT composite phase change materials, we prepared UREA / SAT (1:9~9:1) composite mixtures at different mass ratios and used DSC characterization technology to test the thermal properties of organic-inorganic composite phase change materials at different ratios. When the ratio of SAT to UREA in the system was 1:9~6:4, the prepared CPCM had a higher enthalpy value.
[0046] In order to further screen the best composite ratio, we tested the supercooling of SAT, UREA and UREA / SAT-DHPD composite phase change materials. The raw material UREA has no supercooling, but the supercooling of SAT is extremely high (about 52.0℃); and the most common method to reduce the supercooling of SAT is to add a nucleating agent to it. We added DHPD as a nucleating agent for the UREA / SAT composite system (DHPD content is 1%), and tested the supercooling at different composite ratios. When SAT and UREA each accounted for 50% of the system, the prepared composite system had a low supercooling. Therefore, considering the phase change enthalpy and supercooling results, the UREA / SAT (US) composite ratio of 5:5 was finally selected as the best composite ratio.
[0047] Since solid-liquid phase change materials will produce liquid phase when the phase transition occurs, it will be very easy to leak when it is completely converted to liquid state, which will be unfavorable for its application in the field of building thermal management. Aerogel, as a porous adsorption material, has a series of advantages such as low thermal conductivity, large adsorption capacity and well-developed nanoporosity, and can be used as a supporting skeleton of solid-liquid phase change materials to prevent leakage. Therefore, we innovatively prepared PVA / SiO2 / CNTs composite aerogel. In short, PVA powder was first dissolved in water to form a PVA physical cross-linked network. Secondly, SiO2 aerogel particles and carbon nanotube dispersion were added to form pregel. Finally, PVA / SiO2 / CNTs composite aerogel was prepared by freeze drying technology. PVA was selected as the main network material because of its excellent mechanical properties. PVA chains were cross-linked by hydrogen bonding to form a primary network. At the same time, SiO2 particles and PVA chains also formed a secondary network through hydrogen bonding to improve the mechanical properties of PVA aerogel. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 a is the infrared spectrum of UREA, SAT and US in Example 1; b is the XRD spectrum of UREA, SAT and US in Example 1; c is a comparison chart of melting enthalpy and melting temperature of UREA, SAT and US in Example 1.
[0049] Figure 2 a is the infrared spectra of PVA powder and PVA aerogel in Example 1; b is the infrared spectra of PVA aerogel, SiO2 aerogel and PVA / SiO2 in Example 1; c is the infrared spectra of carbon nanotube solution and PVA / SiO2 / CNTs in Example 1; d is a compressive strength comparison diagram of PVA aerogel, PVA / SiO2 aerogel and PVA / SiO2 / CNTs in Implementation Case 1; e is the pore size distribution diagram corresponding to the nitrogen adsorption-desorption curve of PVA / SiO2 / CNTs composite aerogel in Implementation Case 1; f is the pore size distribution diagram corresponding to the cumulative mercury injection diagram of PVA / SiO2 / CNTs composite aerogel in Implementation Case 1.
[0050] Figure 3 In the figure, a is the image showing the change of the morphology of USD with heating time in implementation case 1; b is the image showing the change of the morphology of USD@PVA / SiO2 / CNTs with heating time.
[0051] Figure 4 Figure a is a digital photo of sodium acetate trihydrate solution with and without urea in Example 1; b is a combustion test diagram of USD@PVA / SiO2 / CNTs at different times; and c is a comparison diagram of USD@PVA / SiO2 / CNTs before and after combustion.
[0052] Figure 5 a is the step cooling curve of SAT in implementation case 1; b is the step cooling curve of UREA in implementation case 1; c is the step cooling curve of US in implementation case 1; d is the step cooling curve of USD in implementation case 1; e is the step cooling curve of USD@PVA / SiO2 / CNTs in implementation case 1.
[0053] Figure 6 a is the DSC endothermic curve of USD and USD@PVA / SiO2 / CNTs in Example 1; b is the DSC endothermic curve of USD@PVA / SiO2 / CNTs in Example 1 after 20, 40, 60, 80 and 100 cycles; c is the phase change temperature and latent heat statistics of USD@PVA / SiO2 / CNTs in Example 1 after different numbers of cycles; d and e are FT-IR and XRD curves of USD, PVA / SiO2 / CNTs aerogel and USD@PVA / SiO2 / CNTs in Example 1, respectively.
[0054] Figure 7 In the figure, a is the temperature rise curve when the foam and phase change material are filled into the simulated building interlayer; b is the temperature drop curve when the foam and phase change material are filled into the simulated building interlayer. DETAILED DESCRIPTION
[0055] The following non-limiting embodiments may enable a person skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.
[0056] The test methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.
[0057] One of the specific implementations:
[0058] Preparation method and application of polyvinyl alcohol-based double-network aerogel-shaped organic-inorganic composite phase change energy storage material, wherein the organic / inorganic composite phase change material is composed of the following components by mass percentage:
[0059] Inorganic solid-liquid phase change material: 30-70wt%;
[0060] Organic solid-liquid phase change material: 40-60wt%;
[0061] Nucleating agent: 0.1-5wt%;
[0062] Porous support material: 5-20wt%.
[0063] The high thermal conductivity flexible phase change material of the present invention preferably consists of the following components by mass percentage:
[0064] Inorganic solid-liquid phase change material: 45.5wt%;
[0065] Organic solid-liquid phase change material: 45.5wt%;
[0066] Nucleating agent: 1.0wt%;
[0067] Porous support material: 8.0 wt%.
[0068] The inorganic phase change material of the present invention is preferably one to three of sodium acetate trihydrate, calcium sulfate dihydrate, potassium aluminum sulfate dodecahydrate, ammonium aluminum sulfate dodecahydrate, magnesium chloride hexahydrate, magnesium sulfate heptahydrate, calcium nitrate tetrahydrate, zinc chloride hexahydrate and sodium thiosulfate pentahydrate.
[0069] The organic phase change material of the present invention is preferably one to three of urea, erythritol, xylitol, mannitol, erythritol, polyethylene glycol, neopentyl glycol, capric acid, lauric acid, palmitic acid and stearic acid.
[0070] In the organic / inorganic solid-liquid phase change material of the present invention, the nucleating agent is preferably 1 to 3 of titanium dioxide, aluminum oxide, zinc oxide, sodium chloride, nanosilver, nanocopper, nanogold, disodium hydrogen phosphate, sodium silicate nonahydrate, silicon dioxide, disodium hydrogen phosphate dodecahydrate, and sodium metasilicate nonahydrate.
[0071] The porous supporting material of the organic / inorganic solid-liquid phase change material of the present invention is preferably polyvinyl alcohol aerogel, and then one to three inorganic nanomaterials such as silicon dioxide, aluminum oxide, titanium dioxide, zirconium dioxide, montmorillonite, carbon nanotubes, nanosilicates, foamed nickel, foamed aluminum, foamed copper, kaolin and mesoporous carbon are added to the polyvinyl alcohol aerogel to form a double network structure for increasing the flame retardant properties and mechanical strength of polyvinyl alcohol.
[0072] A method for preparing a high enthalpy organic / inorganic composite phase change material comprises the following process steps: 4 g urea and 6 g sodium acetate trihydrate are mixed and placed in a 20 mL transparent glass bottle, and the total mass of the mixture is controlled to be 10 g. Secondly, it is placed in a 70°C water bath to dissolve for 120 minutes and then set aside, and finally it is placed under magnetic stirring for 30 minutes and then set aside. Then, 0.1 g disodium hydrogen phosphate dodecahydrate is added to solve the supercooling problem of the composite system, and the mixture is stirred for 30 minutes under magnetic stirring to obtain an organic-inorganic composite phase change material.
[0073] 2.0 g of polyvinyl alcohol powder was dissolved in deionized water at 85°C for half an hour and stirred for 30 minutes. After the polyvinyl alcohol powder was completely dissolved, 1.5 g of silicon dioxide was added and stirred for half an hour. Finally, 15 g of carbon nanotube dispersion was added to prepare PVA / SiO2 / CNTs aerogel.
[0074] Finally, the prepared organic-inorganic composite phase change material was placed in a 100 mL beaker and then placed in a vacuum drying oven at 60°C to melt for later use. Secondly, polyvinyl alcohol-based double network aerogel was added thereto and placed in a vacuum drying oven for vacuum adsorption for 2 hours to obtain a shaped organic / inorganic composite phase change material.
[0075] A polyvinyl alcohol-based double-network aerogel-shaped organic / inorganic composite phase change energy storage material with thermal insulation function, which is filled into the building interlayer, can effectively reduce the building's energy consumption and achieve the purpose of energy saving.
[0076] Example 1
[0077] (1) First, 6g of sodium acetate trihydrate (SAT) and 4g of urea (UREA) were mixed and placed in a 20mL transparent glass bottle, which was placed in a 50℃ water bath to dissolve for 90min and then placed under magnetic stirring for 30min to obtain a composite phase change material (US). Compared with a single organic or inorganic phase change material, the enthalpy value of the composite phase change material remains basically unchanged, but the phase change temperature drops to 29.4℃, which is more suitable for some low-temperature environmental protection and energy-saving fields, such as construction.
[0078] (2) 0.1 g of disodium hydrogen phosphate dodecahydrate was added to the prepared composite phase change material to solve the supercooling problem of the composite system, and the mixture was stirred for 30 minutes under magnetic stirring to obtain an organic-inorganic composite phase change material.
[0079] (3) Dissolve 2.0g of polyvinyl alcohol powder in deionized water at 85°C for half an hour, stir for 30 minutes, and pour the solution into the mold. After freezing the mold in a -20°C refrigerator for 12 hours, put it into a freeze dryer and dry it for 24 hours to obtain polyvinyl alcohol aerogel. The preparation method of polyvinyl alcohol-silica (PVA-SiO2) aerogel is similar to that of polyvinyl alcohol aerogel, except that after the polyvinyl alcohol powder is completely dissolved, 1.5g of silica is added and stirred for half an hour, and other conditions are the same. The preparation of PVA / SiO2 / CNTs aerogel is based on PVA / SiO2 aerogel, and 15g of carbon nanotube dispersion is additionally added. The other conditions remain unchanged to obtain polyvinyl alcohol-based double network aerogel.
[0080] (4) A shaped organic / inorganic composite phase change material was prepared by vacuum impregnation. The preparation method is as follows: first, the prepared organic / inorganic composite phase change material was placed in a 100 mL beaker, and then placed in a vacuum drying oven at 60°C to melt for later use. Secondly, polyvinyl alcohol-based double network aerogel was added thereto, and the mixture was placed in a vacuum drying oven for vacuum adsorption for 2 hours to obtain a shaped organic / inorganic composite phase change material.
[0081] (5) The CPCM was tested for building thermal management using a self-built building model. The building model was composed of a 100*100*60mm hexahedron as an outer model and a 80*80*58mm small hexahedron as an inner model. The thickness of the interlayer between the two models was 10mm. The foam and the shaped phase change material prepared in step 4 were added to the interlayer to test their respective thermal management performance. The specific test process is as follows: We filled the foam and CPCM into the interlayer and the top respectively, and tested the time required for the internal temperature of the test model to rise under outdoor sunlight. Then it was moved to a 0℃ constant temperature and humidity chamber (YH-H, Hangzhou Wujia Machinery Co., Ltd., China) to cool it down (simulating the low temperature outdoor at night), and the time required for cooling was tested to determine the building thermal management performance of the material.
[0082] Example 2
[0083] Urea: 1 g; sodium acetate trihydrate: 9 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0084] Example 3
[0085] Urea: 2 g; sodium acetate trihydrate: 8 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0086] Example 4
[0087] Urea: 3 g; sodium acetate trihydrate: 7 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0088] Example 5
[0089] Urea: 5 g; sodium acetate trihydrate: 5 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0090] Example 6
[0091] Urea: 6 g; sodium acetate trihydrate: 4 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0092] Example 7
[0093] Urea: 7 g; sodium acetate trihydrate: 3 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0094] Example 8
[0095] Urea: 8 g; sodium acetate trihydrate: 2 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1 Example 9
[0096] Urea: 9 g; sodium acetate trihydrate: 1 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0097] Example 10
[0098] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.05 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0099] Embodiment 11
[0100] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.2 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0101] Example 12
[0102] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.3 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0103] Embodiment 13
[0104] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.4 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0105] Embodiment 14
[0106] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.5 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0107] Embodiment 15
[0108] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 1 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0109] Example 16
[0110] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 1.5 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0111] Embodiment 17
[0112] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2.5 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0113] Embodiment 18
[0114] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 3 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0115] Embodiment 19
[0116] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 3.5 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0117] Embodiment 20
[0118] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 4 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0119] Embodiment 21
[0120] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 0.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0121] Embodiment 22
[0122] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 1 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0123] Embodiment 23
[0124] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 2 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0125] Embodiment 24
[0126] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 2.5 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0127] Embodiment 25
[0128] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 3 g; carbon nanotube dispersion: 15 g. Other conditions are the same as those in Example 1.
[0129] Embodiment 26
[0130] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 0 g. Other conditions are the same as those in Example 1.
[0131] Embodiment 27
[0132] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 5 g. Other conditions are the same as those in Example 1.
[0133] Embodiment 28
[0134] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 10 g. Other conditions are the same as those in Example 1.
[0135] Embodiment 29
[0136] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 20 g. Other conditions are the same as those in Example 1.
[0137] Embodiment 30
[0138] Urea: 4 g; sodium acetate trihydrate: 6 g; disodium hydrogen phosphate dodecahydrate: 0.1 g; polyvinyl alcohol: 2 g; silicon dioxide: 1.5 g; carbon nanotube dispersion: 30 g. Other conditions are the same as those in Example 1.
[0139] From the infrared spectrum of the material ( Figure 1 In a), it can be seen that all the diffraction peaks of UREA and SAT appear in the US infrared spectrum, and no new diffraction peaks appear, which indicates that UREA and SAT are only combined by physical action and no chemical reaction occurs.
[0140] From the XRD characterization of the material ( Figure 1 In b), it can be seen that the diffraction peaks of the obtained US retain all the characteristic diffraction peaks of UREA and SAT, and no new characteristic peaks appear, but the intensity of the peaks changes. This indicates that US forms a eutectic structure.
[0141] From the DSC comparison chart of the materials ( Figure 1 In c), it can be seen that the phase change temperature of the eutectic phase change material is reduced to 29.4°C compared with 57.5°C of the raw materials SAT and 130.4°C of UREA, making it more suitable for the construction field.
[0142] From the infrared spectrum of the material ( Figure 2 As can be seen in a), PVA powder and PVA aerogel show typical broad hydroxyl absorption peaks at 3200-3600 cm-1, which is caused by extensive intermolecular and intramolecular hydrogen bonding interactions of PVA.
[0143] From the infrared spectrum of the material ( Figure 2 As can be seen in Figure b), compared with PVA aerogel, the hydroxyl absorption vibration peak in PVA / SiO2 composite aerogel has a red shift, which indicates that hydrogen bonding forces are formed between the hydroxyl in PVA and the Si-OH in silica, causing it to shift. Finally, the infrared spectra of CNTs dispersion and PVA / SiO2 / CNTs were tested, and the results are shown in Figure 2. Figure 2 As shown in Figure c, it can be seen from the figure that the addition of CNTs dispersion did not form a new characteristic peak, which indicates that the two are only combined through physical action and no new chemical force is formed.
[0144] Figure 2 Figure d is a comparison of the compressive strength of PVA aerogel, PVA / SiO2 aerogel and PVA / SiO2 / CNTs. It can be seen from the figure that the compressive strength of PVA / SiO2 and PVA / SiO2 / CNTs aerogels is twice that of PVA aerogel. This is attributed to the double cross-linked network formed between PVA and PVA and between PVA and SiO2 particles, which significantly enhances the mechanical properties of the composite aerogel material.
[0145] In order to analyze the pore structure information of PVA / SiO2 / CNTs composite aerogel, we used nitrogen physical adsorption and fully automatic mercury intrusion analysis to perform full pore size analysis. The results are as follows: Figure 2 As shown in e. The results show that PVA / SiO2 / CNTs aerogel has a small amount of mesopores, distributed between 20 and 50 nm. Figure 2 f It can be seen that the pore sizes of PVA / SiO2 / CNTs aerogel are mainly distributed in 100-4000nm and 5000-20000nm, which indicates that PVA / SiO2 / CNTs composite aerogel is mainly composed of macropores. The developed pore structure is conducive to the adsorption of a large amount of phase change materials, thereby preparing phase change aerogel composite materials.
[0146] Figure 3 In the figure, a is USD, and b is the change of USD@PVA / SiO2 / CNTs with heating time. It can be seen from the figure that USD began to leak after about 20 minutes of heating, and completely leaked after 90 minutes. However, USD@PVA / SiO2 / CNTs phase change aerogel did not leak even after being heated on a 50°C heating plate for 120 minutes, which shows that it has excellent shape stability.
[0147] from Figure 4 Figure a shows the sodium acetate trihydrate solution with and without urea. It can be seen from the figure that SAT has a phase separation problem. After the composite system is formed, the composite system can effectively solve its phase separation problem. Figure 4 It can be seen from the graph that USD@PVA / SiO2 / CNTs cannot be burned after being burned by an alcohol lamp for one minute, and no dripping of the molten material is observed after burning, which proves that USD@PVA / SiO2 / CNTs has good flame retardant properties.
[0148] Figure 5a is the step-cooling curve of SAT in implementation case 1; b is the step-cooling curve of UREA in implementation case 1; c is the step-cooling curve of US in implementation case 1; d is the step-cooling curve of USD in implementation case 1; e is the step-cooling curve of USD@PVA / SiO2 / CNTs in implementation case 1. From ae, we can see that when the two form a composite system, the supercooling degree is reduced from 52.0℃ to 11.3℃; to further reduce its supercooling degree, we added DHPD nucleating agent to it, and the supercooling degree was reduced to 7.3℃; finally, we used PVA / SiO2 / CNTs aerogel to shape and encapsulate it, and it can be seen that the supercooling degree of USD@PVA / SiO2 / CNTs further dropped to 5.1℃.
[0149] from Figure 6 Figure a is the DSC endothermic curve of USD and USD@PVA / SiO2 / CNTs. It can be seen that the enthalpy value of USD@PVA / SiO2 / CNTs is as high as 194.3 J / g, which is higher than the previously reported composite phase change materials used in building thermal management, indicating that it has great potential for application in the field of building thermal management. Figure 6 Figures bc in the figure are the results of 100 thermal cycle tests on USD@PVA / SiO2 / CNTs. It can be seen from the figure that after 100 hot and cold cycles, the latent heat and phase change temperature of USD@PVA / SiO2 / CNTs in the melting and solidification process have hardly changed, which indicates that the prepared CPCM has good cycle stability.
[0150] Figure 6 Figure 1 shows the FT-IR and XRD characterization tests of USD, PVA / SiO2 / CNTs and USD@PVA / SiO2 / CNTs. From the results, it can be seen that the two are only physically combined, and no chemical reaction occurs.
[0151] Considering the excellent cycle stability, low supercooling and high enthalpy value of USD@PVA / SiO2 / CNTs, we chose to conduct actual application tests on it. The results are as follows: Figure 7As shown in ab. From the results, the indoor heating rate of the foam group is much faster than that of the experimental group. When both groups of models were moved to a constant temperature and humidity chamber at 0°C (simulating the low temperature outdoor at night), the indoor temperature of the foam group dropped instantly, while the temperature of the CPCM group changed slowly. The time for the CPCM group to maintain the indoor temperature above 18°C was 8.7 times that of the blank group. This shows that the composite phase change material has phase change heat release in this process, maintaining the room temperature relatively stable, reducing the fluctuation amplitude of indoor air temperature, and increasing body surface comfort. On the whole, CPCM can significantly delay the heating and cooling time inside the building, has good building thermal management capabilities, and has great practical application value.
[0152] In order to determine the optimal ratio of UREA / SAT composite phase change materials, we prepared UREA / SAT (1:9~9:1) composite mixtures at different mass ratios, and used DSC characterization technology to test the thermal properties of organic-inorganic composite phase change materials at different ratios. As shown in Table 1, when the ratio of SAT to UREA in the system is 1:9~6:4, the prepared CPCM enthalpy value is higher.
[0153] In order to further screen the best composite ratio, we tested the supercooling of SAT, UREA and UREA / SAT-DHPD composite phase change materials. The raw material UREA has no supercooling, but the supercooling of SAT is extremely high (about 52.0℃); and the most common method to reduce the supercooling of SAT is to add a nucleating agent to it. We added DHPD as a nucleating agent for the UREA / SAT composite system (DHPD content is 1%), and tested the supercooling at different composite ratios. As shown in Table 1, when SAT and UREA each account for 50% of the system, the prepared composite system has a low supercooling. Therefore, considering the phase change enthalpy and supercooling results, the UREA / SAT (US) composite ratio of 5:5 was finally selected as the best composite ratio.
[0154] Table 1 US (1% DHPD) at different ratios
[0155]
[0156]
[0157] The preparation method of the phase change material also includes:
[0158] Examples 31-60
[0159] Barium hydroxide octahydrate is used instead of sodium acetate trihydrate as the phase change material to obtain the corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0160] Examples 61-90
[0161] Magnesium chloride hexahydrate is used instead of sodium acetate trihydrate as the phase change material to obtain the corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0162] Examples 91-120
[0163] Calcium chloride hexahydrate is used instead of sodium acetate trihydrate as the phase change material to obtain the corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0164] Examples 121-150
[0165] Magnesium sulfate heptahydrate is used instead of sodium acetate trihydrate as the phase change material to obtain the corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0166] Examples 151-180
[0167] Sodium carbonate decahydrate is used instead of sodium acetate trihydrate as the phase change material to obtain the corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0168] Examples 181-210
[0169] Disodium hydrogen phosphate dodecahydrate is used instead of sodium acetate trihydrate as the phase change material to obtain the corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0170] Embodiments 211-240
[0171] Sodium sulfate decahydrate is used instead of sodium acetate trihydrate as the phase change material to obtain the corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0172] Embodiments 241-270
[0173] Sodium thiosulfate pentahydrate is used instead of sodium acetate trihydrate as the phase change material to obtain the corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0174] Embodiment 271-300
[0175] Erythritol is used instead of urea as the phase change material to obtain the corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0176] Examples 301-330
[0177] Xylitol was used as the phase change material instead of urea to obtain the corresponding high enthalpy organic / inorganic composite phase change material, and other conditions were consistent with those of Example 1-30.
[0178] Examples 331-360
[0179] Mannitol was used instead of urea as the phase change material to obtain the corresponding high enthalpy organic / inorganic composite phase change material, and other conditions were consistent with those of Example 1-30.
[0180] Examples 361-390
[0181] Erythritol is used instead of urea as the phase change material to obtain the corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0182] Examples 391-420
[0183] By using polyethylene glycol instead of urea as the phase change material, the corresponding high enthalpy organic / inorganic composite phase change material is obtained, and other conditions are consistent with those of Example 1-30.
[0184] Examples 421-450
[0185] Neopentyl glycol is used instead of urea as the phase change material to obtain the corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0186] Examples 451-480
[0187] Decanoic acid is used instead of urea as the phase change material to obtain the corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0188] Examples 481-510
[0189] The corresponding high enthalpy organic / inorganic composite phase change material is obtained by using lauric acid instead of urea as the phase change material, and other conditions are consistent with those of Example 1-30.
[0190] Examples 511-540
[0191] Palmitic acid is used instead of urea as the phase change material to obtain the corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0192] Examples 541-570
[0193] By using stearic acid instead of urea as the phase change material, the corresponding high enthalpy organic / inorganic composite phase change material is obtained, and other conditions are consistent with those of Example 1-30.
[0194] Examples 571-600
[0195] Titanium dioxide is used as a nucleating agent instead of disodium hydrogen phosphate dodecahydrate to obtain a corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0196] Examples 601-630
[0197] Alumina is used as a nucleating agent instead of disodium hydrogen phosphate dodecahydrate to obtain a corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0198] Examples 631-660
[0199] Zinc oxide is used as a nucleating agent instead of disodium hydrogen phosphate dodecahydrate to obtain a corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0200] Examples 661-690
[0201] Sodium chloride is used as a nucleating agent instead of disodium hydrogen phosphate dodecahydrate to obtain a corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0202] Examples 691-720
[0203] Nanosilver is used as a nucleating agent instead of disodium hydrogen phosphate dodecahydrate to obtain a corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0204] Examples 721-750
[0205] Nano copper is used as a nucleating agent instead of disodium hydrogen phosphate dodecahydrate to obtain a corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0206] Examples 751-780
[0207] Nano-gold was used as a nucleating agent instead of disodium hydrogen phosphate dodecahydrate to obtain a corresponding high enthalpy organic / inorganic composite phase change material, and other conditions were consistent with those of Example 1-30.
[0208] Examples 781-810
[0209] Disodium hydrogen phosphate is used as a nucleating agent instead of disodium hydrogen phosphate dodecahydrate to obtain a corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0210] Embodiments 811-840
[0211] Sodium silicate nonahydrate was used as a nucleating agent instead of disodium hydrogen phosphate dodecahydrate to obtain a corresponding high enthalpy organic / inorganic composite phase change material, and other conditions were consistent with those of Example 1-30.
[0212] Embodiments 841-870
[0213] Silicon dioxide is used instead of disodium hydrogen phosphate dodecahydrate as a nucleating agent to obtain a corresponding high enthalpy organic / inorganic composite phase change material, and other conditions are consistent with those of Example 1-30.
[0214] Embodiment 871-900
[0215] Sodium metasilicate nonahydrate was used as a nucleating agent instead of disodium hydrogen phosphate dodecahydrate to obtain a corresponding high enthalpy organic / inorganic composite phase change material, and other conditions were consistent with those of Example 1-30.
[0216] Examples 901-930
[0217] Alumina is used instead of silica as the polyvinyl alcohol-based double network aerogel, which is cross-linked with polyvinyl alcohol through supramolecular forces to form a stable double network structure for increasing the flame retardancy and mechanical strength of polyvinyl alcohol. Other conditions are consistent with Examples 1-30.
[0218] Examples 931-960
[0219] Titanium dioxide is used instead of silicon dioxide as the polyvinyl alcohol-based double network aerogel, which is cross-linked with polyvinyl alcohol through supramolecular forces to form a stable double network structure for increasing the flame retardant properties and mechanical strength of polyvinyl alcohol. Other conditions are consistent with Examples 1-30.
[0220] Examples 961-990
[0221] Zirconium dioxide is used instead of silicon dioxide as the polyvinyl alcohol-based double network aerogel, which is cross-linked with polyvinyl alcohol through supramolecular forces to form a stable double network structure for increasing the flame retardant properties and mechanical strength of polyvinyl alcohol. Other conditions are consistent with Examples 1-30.
[0222] Examples 991-1020
[0223] Montmorillonite is used instead of silica as the polyvinyl alcohol-based double network aerogel, which is cross-linked with polyvinyl alcohol through supramolecular forces to form a stable double network structure for increasing the flame retardant properties and mechanical strength of polyvinyl alcohol. Other conditions are consistent with Examples 1-30.
[0224] Embodiments 1021-1050
[0225] Nanosilicate is used instead of silicon dioxide as the polyvinyl alcohol-based double network aerogel, which is cross-linked with polyvinyl alcohol through supramolecular forces to form a stable double network structure for increasing the flame retardancy and mechanical strength of polyvinyl alcohol. Other conditions are consistent with Examples 1-30.
[0226] Examples 1051-1080
[0227] Nickel foam is used instead of silicon dioxide as the polyvinyl alcohol-based double network aerogel, which is cross-linked with polyvinyl alcohol through supramolecular forces to form a stable double network structure for increasing the flame retardant properties and mechanical strength of polyvinyl alcohol. Other conditions are consistent with Examples 1-30.
[0228] Embodiments 1081-1110
[0229] Foamed aluminum is used instead of silicon dioxide as the polyvinyl alcohol-based double network aerogel, which is cross-linked with polyvinyl alcohol through supramolecular forces to form a stable double network structure for increasing the flame retardancy and mechanical strength of polyvinyl alcohol. Other conditions are consistent with Examples 1-30.
[0230] Embodiments 1111-1140
[0231] Copper foam is used instead of silicon dioxide as the polyvinyl alcohol-based double network aerogel, which is cross-linked with polyvinyl alcohol through supramolecular forces to form a stable double network structure for increasing the flame retardant properties and mechanical strength of polyvinyl alcohol. Other conditions are consistent with Examples 1-30.
[0232] Embodiments 1141-1170
[0233] Kaolin is used instead of silica as the polyvinyl alcohol-based double network aerogel, which is cross-linked with polyvinyl alcohol through supramolecular forces to form a stable double network structure for increasing the flame retardant properties and mechanical strength of polyvinyl alcohol. Other conditions are consistent with Examples 1-30.
[0234] Embodiment 1171-1200
[0235] Mesoporous carbon is used instead of silica as the polyvinyl alcohol-based double network aerogel, which is cross-linked with polyvinyl alcohol through supramolecular forces to form a stable double network structure for increasing the flame retardant properties and mechanical strength of polyvinyl alcohol. Other conditions are consistent with Examples 1-30.
[0236] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. Polyvinyl alcohol-based double network aerogel shaped composite phase change energy storage material, Features: The material includes an inorganic solid-liquid phase change material, an organic solid-liquid phase change material, a nucleating agent and a polyvinyl alcohol-based double-network aerogel supporting material; by mass percentage: Inorganic solid-liquid phase change material 30~70wt%; Organic solid-liquid phase change material 40~60wt%; Nucleating agent 0.1~5wt%; Polyvinyl alcohol-based double network aerogel 5~20wt%; The polyvinyl alcohol-based double network aerogel is prepared by adding inorganic nanomaterials into polyvinyl alcohol aerogel. The inorganic nanomaterials are cross-linked with the polyvinyl alcohol through supramolecular forces to form a stable double network structure.
2. The phase change energy storage material according to claim 1, Features: The inorganic solid-liquid phase change material is one to three of sodium acetate trihydrate, calcium sulfate dihydrate, potassium aluminum sulfate dodecahydrate, ammonium aluminum sulfate dodecahydrate, magnesium chloride hexahydrate, magnesium sulfate heptahydrate, calcium nitrate tetrahydrate, zinc chloride hexahydrate and sodium thiosulfate pentahydrate.
3. The phase change energy storage material according to claim 1, Features: The organic solid-liquid phase change material is one to three of urea, erythritol, xylitol, mannitol, erythritol, polyethylene glycol, neopentyl glycol, capric acid, lauric acid, palmitic acid, and stearic acid.
4. The phase change energy storage material according to claim 1, Features: The nucleating agent is one to three of titanium dioxide, aluminum oxide, zinc oxide, sodium chloride, nano silver, nano copper, nano gold, disodium hydrogen phosphate, sodium silicate nonahydrate, silicon dioxide, disodium hydrogen phosphate dodecahydrate and sodium metasilicate nonahydrate.
5. The phase change energy storage material according to claim 1, It is characterized in that The inorganic nanomaterials are one to three of silicon dioxide, aluminum oxide, titanium dioxide, zirconium dioxide, montmorillonite, carbon nanotubes, nanosilicates, foamed nickel, foamed aluminum, foamed copper, kaolin and mesoporous carbon.
6. A method for preparing the phase change energy storage material according to any one of claims 1 to 5, It is characterized in that The following steps are involved: (1) First, the inorganic hydrated salt phase change material is heated in a water bath to melt and stirred to obtain a hydrated salt solution; (2) dissolving and mixing the organic phase change material and the above-mentioned hydrated salt solution under heating conditions in a water bath to form an organic-inorganic composite phase change material; adding a nucleating agent thereto to reduce the supercooling problem of the composite phase change material, and stirring evenly to obtain an organic / inorganic composite phase change material; (3) dissolving polyvinyl alcohol powder in deionized water, adding inorganic nanomaterials after stirring or evenly mixing the inorganic nanomaterials, and then pouring the solution into a mold; freezing the mold in a refrigerator, and then drying it in a freeze dryer to obtain a polyvinyl alcohol-based double network aerogel; (4) Preparing a shaped organic / inorganic composite phase change material by a vacuum impregnation method: melting the above organic / inorganic composite phase change material; adding polyvinyl alcohol-based double network aerogel thereto for encapsulation; and obtaining a shaped organic / inorganic composite phase change material after vacuum impregnation.
7. Application of the phase change energy storage material according to any one of claims 1 to 6, Features: The phase change energy storage material is used in building thermal insulation thermal management.
8. Application of the phase change energy storage material according to claim 6, Features: The temperature range of application of the phase change energy storage material is 19-40°C.
Citation Information
Cited By
Novel phase change energy lattice and preparation method thereof
CN119570455A
A phase change energy lattice and method of making the same
CN119570455B
High-enthalpy-value phase-change gel material for cold-chain transportation and preparation method of high-enthalpy-value phase-change gel material
CN119979127A
Flame-retardant composite phase change material as well as preparation method and application thereof
CN120209790A
A flame retardant composite phase change material and its preparation method and application
CN120209790B