High-latent-heat liquid metal phase change microcapsule as well as preparation method and application thereof

Through simple preparation methods and cheap raw materials, high latent heat liquid metal phase change microcapsules are prepared, which solves the problem of high production cost of liquid metal microcapsules in the prior art, and realizes low-cost and high latent heat performance microcapsules, suitable for electronics Thermal management of the product.

CN118879284AActive Publication Date: 2024-11-01SHANDONG INST OF ADVANCED TECH
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411176907.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-01
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The preparation of existing liquid metal microcapsules has huge raw materials and complex preparation processes, which leads to high production costs and is difficult to meet the needs of electronic products.

Method used

Using a simple preparation method, using cheap and easy-to-get raw materials, including liquid metal, nucleating agent, surfactant, shell material precursor and catalyst, high latent heat liquid metal phase change microcapsules are prepared by stirring, micronization and reaction steps. Use inorganic shell materials to improve thermal conductivity and protect liquid metals.

Benefits of technology

It realizes the preparation of liquid metal microcapsules with low cost and low raw material consumption, has excellent latent heat performance, can effectively reduce the working temperature of components, and improve the stability and reliability of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005010956730000011
    Figure HDA0005010956730000011
Patent Text Reader

Abstract

The invention provides a high-latent-heat liquid metal phase change microcapsule and a preparation method and application thereof. The high-latent-heat liquid metal phase change microcapsule is prepared from the following raw materials in parts by mass: 400 to 600 parts of liquid metal, 1 to 5 parts of a nucleating agent, 20 to 50 parts of a surfactant, 30 to 60 parts of a shell material precursor and 1500 to 2000 parts of a catalyst. The preparation method is simple, raw materials are cheap and easy to obtain, consumption of the raw materials is low, cost is low, and market requirements can be met; the obtained liquid metal phase change microcapsule has excellent latent heat performance, the working temperature of components can be effectively reduced, and the stability and reliability of instruments and equipment are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of thermal management, and in particular to a high latent heat liquid metal phase change microcapsule and a preparation method and application thereof. Background Art

[0002] With the development of electronic technology and the integration of electronic products, the heat flux density in electronic components is getting higher and higher, and the heat dissipation requirements of electronic components are also getting higher and higher. If the operating temperature of components in electronic equipment is too high, it will reduce the life and performance of the equipment. Phase change microcapsules can store or release a large amount of latent heat and fill the interface gaps during the phase change process, effectively reducing the operating temperature of components and improving the stability and reliability of instruments and equipment. They are widely used in thermal management of electronic devices.

[0003] Chinese patent document CN104449588A discloses a low melting point metal endothermic solution, in which the dispersed phase in the dispersion system is a phase change microcapsule, and the dispersion medium is oil, water or alcohol. The phase change microcapsule is made of a high molecular polymer as the wall material and a low melting point metal as the core material. The low melting point metal has a high phase change latent heat and thermal conductivity. The low melting point metal endothermic solution of the invention can quickly absorb the heat of a high temperature object (liquid or solid), so that the high temperature object can be quickly cooled to the required temperature. However, the wall material of the invention is a high molecular polymer, which has a very poor thermal conductivity, which seriously hinders heat transfer.

[0004] At present, the preparation of liquid metal microcapsules has problems such as huge consumption of raw materials and complex preparation process, which leads to high production cost of liquid metal microcapsules and high price, which is difficult to meet the needs of a large number of electronic products. Therefore, it is of great significance to provide a liquid metal microcapsule with cheap and easy-to-obtain raw materials, simple preparation process, low cost and excellent latent heat performance. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a high latent heat liquid metal phase change microcapsule and its preparation method and application. The preparation method of the present invention is simple, the raw materials are cheap and easy to obtain, the raw material consumption is small, the cost is low, and the market demand can be met; the obtained liquid metal phase change microcapsule has excellent latent heat performance, can effectively reduce the operating temperature of components, and improve the stability and reliability of instruments and equipment.

[0006] The technical solution of the present invention is as follows:

[0007] A high latent heat liquid metal phase change microcapsule is prepared by comprising the following raw materials in parts by weight: 400-600 parts of liquid metal, 1-5 parts of nucleating agent, 20-50 parts of surfactant, 30-60 parts of shell material precursor, and 1500-2000 parts of catalyst.

[0008] Preferably according to the present invention, the high latent heat liquid metal phase change microcapsules are prepared by including the following raw materials in parts by weight: liquid metal: 450-550 parts, nucleating agent: 2-4.2 parts, surfactant: 25-40 parts, shell material precursor: 45-50 parts, catalyst: 1800-1850 parts.

[0009] Preferably, the high latent heat liquid metal phase change microcapsules are prepared by including the following raw materials in parts by weight: liquid metal: 500 parts, nucleating agent: 2.5 parts, surfactant: 30 parts, shell material precursor: 46 parts, catalyst: 1820 parts.

[0010] Preferably according to the present invention, the liquid metal is one or a combination of two or more of cesium, gallium, indium or tin.

[0011] Preferably according to the present invention, the nucleating agent is one or a combination of two or more of iron, copper, tellurium dioxide, calcium oxide or magnesium oxide.

[0012] According to the present invention, preferably, the surfactant is one or a combination of two or more of cetyltrimethylammonium bromide, dodecyldimethylamine oxide, dopamine hydrochloride or sodium dodecyl sulfate.

[0013] Preferably according to the present invention, the shell material precursor is one or a combination of two or more of tetraethyl orthosilicate, calcium hydroxide, methyl silicate or triethoxysilane.

[0014] According to the present invention, the catalyst is preferably silver hydroxide, sodium hydroxide, sodium bicarbonate or ammonia water with a mass concentration of 20-30%, or a combination of two or more thereof.

[0015] The method for preparing the high latent heat liquid metal phase change microcapsules comprises the following steps:

[0016] (1) stirring and mixing the liquid metal and the nucleating agent uniformly, and then adding them dropwise into the surfactant aqueous solution to obtain a mixed solution through micronization;

[0017] (2) uniformly mixing the shell material precursor and the catalyst to obtain a shell layer reactant;

[0018] (3) The mixed solution obtained in step (1) and the shell layer reactant obtained in step (2) are mixed, reacted, filtered, washed, and dried to obtain high latent heat liquid metal phase change microcapsules.

[0019] Preferably, according to the present invention, in step (1), the stirring and mixing of the liquid metal and the nucleating agent is carried out in a planetary centrifugal mixer, the stirring and mixing time is 10-20 minutes, the stirring and mixing temperature is room temperature, and the stirring rate is 800-2000 r / min.

[0020] Preferably according to the present invention, in step (1), the mass concentration of the surfactant aqueous solution is 5-15%.

[0021] Preferably according to the present invention, in step (1), the micronization is carried out under ultrasonic conditions; the ultrasonic time is 1-2h, the ultrasonic power is 100-800W, preferably the ultrasonic power is 400-500W, and more preferably the ultrasonic power is 400W.

[0022] Preferably, according to the present invention, in step (2), the mixture of the shell material precursor and the catalyst is stirred at room temperature for 15-25 min at a stirring rate of 500-2000 r / min.

[0023] Preferably, in step (3), the reaction temperature is room temperature, the reaction time is 1-2 h, and the reaction is carried out under stirring at a stirring rate of 800-2000 r / min.

[0024] Application of the above-mentioned high latent heat liquid metal phase change microcapsules in thermal management materials and devices.

[0025] The technical features and beneficial effects of the present invention are as follows:

[0026] 1. The preparation method of the present invention is simple, the raw materials are cheap and easily available, the raw material consumption is small, the cost is low, and the market demand can be met.

[0027] 2. The liquid metal selected in the present invention has a large latent heat value and can absorb a large amount of heat during the phase change process. The shell material selected in the present invention is an inorganic material, which has a relatively high thermal conductivity compared with the microcapsules prepared from the existing organic shell materials, and is more conducive to heat transfer. The nucleating agent added in the present invention reduces the supercooling degree and significantly increases the latent heat of the microcapsule phase change, but when a trace or excessive amount of nucleating agent is added, there is no effect of reducing supercooling.

[0028] 3. In the preparation method of the present invention, the ultrasonic power of micronization has a great influence on the performance of the microcapsules. When the power is too low, the liquid metal cannot be effectively dispersed into tiny droplets. When the power is too high, the particle size of the obtained liquid metal microcapsules is too small and the heat storage capacity is weak.

[0029] 4. The inorganic shell of the microcapsule of the present invention can protect the liquid metal inside, solve the problem of easy oxidation and leakage, greatly reduce the loss of liquid metal, and reduce the cost. The liquid metal phase change microcapsule of the present invention has excellent latent heat performance, with a latent heat value of up to 46.7 J / g, which can effectively reduce the operating temperature of components and improve the stability and reliability of instruments and equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1It is a comparison diagram of the DSC curves of the liquid metal phase change microcapsules prepared in Examples 2-3 of the present invention and Comparative Examples 1-2. DETAILED DESCRIPTION

[0031] The present invention is further described below with reference to specific embodiments, but is not limited thereto.

[0032] Meanwhile, the experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0033] Example 1

[0034] A high latent heat liquid metal phase change microcapsule is prepared by including the following raw materials in parts by mass: 500 parts of metal gallium (liquid), 2.5 parts of tellurium dioxide as a nucleating agent, 30 parts of dopamine hydrochloride as a surfactant, 46 parts of tetraethyl orthosilicate as a shell material precursor, and 1820 parts of ammonia water with a catalyst mass concentration of 25%.

[0035] The method for preparing the high latent heat liquid metal phase change microcapsules comprises the following steps:

[0036] S1. Pour 500 parts of liquid metal gallium and 2.5 parts of tellurium dioxide into a planetary centrifugal mixer and stir at room temperature at 2000r / min for 10min;

[0037] S2. Take 30 parts of dopamine hydrochloride and dissolve it in 300 parts of water to prepare an aqueous surfactant solution;

[0038] S3. The mixture (liquid state) obtained in step S1 is added dropwise to the solution obtained in step S2, and ultrasonic micronization is performed at a power of 500 W for 1 h;

[0039] S4. Mix 46 parts of tetraethyl orthosilicate with 1820 parts of aqueous ammonia and stir at room temperature for 20 min at 600 r / min;

[0040] S5. The solution obtained in step S3 above was mixed with the solution obtained in step S4 and stirred at room temperature for 2 h at 1200 r / min;

[0041] S6. Filter, wash and dry the mixture obtained in the reaction of step S5 to finally obtain high latent heat liquid metal microcapsules.

[0042] The latent heat value of the liquid metal phase change microcapsules prepared in this embodiment is 38.5 J / g.

[0043] Example 2

[0044] A high latent heat liquid metal phase change microcapsule, the raw material composition is as described in Example 1;

[0045] The method for preparing the high latent heat liquid metal phase change microcapsules is as described in Example 1, except that the ultrasonic power in step S3 is 400 W; the other steps and conditions are the same as in Example 1.

[0046] The liquid metal phase-change microcapsules prepared in this embodiment have a melting point of 30.9° C. and a latent heat value of 46.7 J / g.

[0047] Example 3

[0048] A high latent heat liquid metal phase change microcapsule is prepared by including the following raw materials in parts by mass: 500 parts of metal gallium (liquid), 4.2 parts of tellurium dioxide as a nucleating agent, 30 parts of dopamine hydrochloride as a surfactant, 46 parts of tetraethyl orthosilicate as a shell material precursor, and 1820 parts of ammonia water with a catalyst mass concentration of 25%.

[0049] The preparation method of the high latent heat liquid metal phase change microcapsules is as described in Example 2.

[0050] The liquid metal phase-change microcapsules prepared in this embodiment have a melting point of 30.7° C. and a latent heat value of 34.7 J / g.

[0051] Comparative Example 1

[0052] A high latent heat liquid metal phase change microcapsule, the raw material composition is as described in Example 2, except that: no nucleating agent is added; the other raw material compositions are the same as Example 2.

[0053] The preparation method of the high latent heat liquid metal phase change microcapsules is as described in Example 2, except that no nucleating agent is added; the other steps and conditions are the same as in Example 2.

[0054] Comparative Example 2

[0055] A high latent heat liquid metal phase change microcapsule is prepared by including the following raw materials in parts by mass: 500 parts of metal gallium (liquid), 5.8 parts of tellurium dioxide as a nucleating agent, 30 parts of dopamine hydrochloride as a surfactant, 46 parts of tetraethyl orthosilicate as a shell material precursor, and 1820 parts of ammonia water with a catalyst mass concentration of 25%.

[0056] The preparation method of the high latent heat liquid metal phase change microcapsules is as described in Example 2.

[0057] Test example

[0058] The DSC curves of the liquid metal phase change microcapsules prepared in Example 2-3 and Comparative Example 1-2 are as follows: Figure 1 When no nucleating agent is added or when the nucleating agent is excessive, the microcapsules have no endothermic peaks. The former is due to the nano effect of the liquid metal, while the latter is because the excessive nucleating agent destroys the original lattice structure of the liquid metal, causing its properties to change.

Claims

1. A high latent heat liquid metal phase change microcapsule, characterized in that: The preparation method comprises the following raw materials in parts by weight: 400-600 parts of liquid metal, 1-5 parts of nucleating agent, 20-50 parts of surfactant, 30-60 parts of shell material precursor and 1500-2000 parts of catalyst.

2. The high latent heat liquid metal phase change microcapsule according to claim 1, characterized in that: The high latent heat liquid metal phase change microcapsules are prepared by including the following raw materials in parts by weight: liquid metal: 450-550 parts, nucleating agent: 2-4.2 parts, surfactant: 25-40 parts, shell material precursor: 45-50 parts, catalyst: 1800-1850 parts.

3. The high latent heat liquid metal phase change microcapsule according to claim 1, characterized in that: The liquid metal is one or a combination of two or more of cesium, gallium, indium or tin.

4. The high latent heat liquid metal phase change microcapsule according to claim 1, characterized in that: The nucleating agent is one or a combination of two or more of iron, copper, tellurium dioxide, calcium oxide or magnesium oxide.

5. The high latent heat liquid metal phase change microcapsule according to claim 1, characterized in that: Includes one or more of the following conditions: i. The surfactant is one or a combination of two or more of cetyltrimethylammonium bromide, dodecyldimethylamine oxide, dopamine hydrochloride or sodium dodecyl sulfate; ii. The shell material precursor is one or a combination of two or more of tetraethyl orthosilicate, calcium hydroxide, methyl silicate or triethoxysilane; iii. The catalyst is one or a combination of two or more of silver hydroxide, sodium hydroxide, sodium bicarbonate or ammonia water with a mass concentration of 20-30%.

6. The method for preparing the high latent heat liquid metal phase change microcapsules according to any one of claims 1 to 5, comprising the steps of: (1) stirring and mixing the liquid metal and the nucleating agent uniformly, and then adding them dropwise into the surfactant aqueous solution to obtain a mixed solution through micronization; (2) uniformly mixing the shell material precursor and the catalyst to obtain a shell layer reactant; (3) The mixed solution obtained in step (1) and the shell layer reactant obtained in step (2) are mixed, reacted, filtered, washed, and dried to obtain high latent heat liquid metal phase change microcapsules.

7. The method for preparing high latent heat liquid metal phase change microcapsules according to claim 6, characterized in that: In step (1), the stirring and mixing of the liquid metal and the nucleating agent is carried out in a planetary centrifugal mixer, the stirring and mixing time is 10-20 minutes, the stirring and mixing temperature is room temperature, and the stirring rate is 800-2000r / min; preferably, in step (1), the mass concentration of the surfactant aqueous solution is 5-15%.

8. The method for preparing high latent heat liquid metal phase change microcapsules according to claim 6, characterized in that: In step (1), the micronization is carried out under ultrasonic conditions; the ultrasonic time is 1-2h, the ultrasonic power is 100-800W, preferably the ultrasonic power is 400-500W, and more preferably the ultrasonic power is 400W.

9. The method for preparing high latent heat liquid metal phase change microcapsules according to claim 6, characterized in that: In step (2), the mixture of the shell material precursor and the catalyst is stirred at room temperature for 15-25 minutes at a stirring rate of 500-2000 r / min; preferably, in step (3), the reaction temperature is room temperature, the reaction time is 1-2 hours, and the reaction is carried out under stirring conditions at a stirring rate of 800-2000 r / min.

10. Use of the high latent heat liquid metal phase change microcapsule according to any one of claims 1 to 5 in thermal management materials and devices.

Citation Information

Patent Citations

  • Composite phase change thermal storage material, microcapsule and preparation method thereof

    CN106701032A

  • Metal and alloy phase change energy storage microcapsule and preparation method thereof

    CN106916573A

  • Low-temperature organic phase change energy storage material, preparation method and applications thereof

    CN110204446A

  • Low-temperature composite phase-change energy storage material as well as preparation method and application thereof

    CN111100606A

  • Metal phase change microcapsule with thermal expansion cavity and preparation method of metal phase change microcapsule

    CN112473579A