Suspended thickening agent for fracturing and preparation method thereof

By using a suspension thickener in the fracturing fluid, combined with acrylamide polymers and clay stabilizers, the problems of complex preparation process and insufficient performance in the prior art are solved, and efficient construction in high-temperature deep wells are achieved and low environmental damage.

CN118879299APending Publication Date: 2024-11-01SHAANXI UNIV OF SCI & TECH

Patent Information

Application Number
CN202410836850.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The preparation process of existing fracturing fluid is complex, the raw material cost is high, and the performance is insufficient in unconventional reservoirs with high temperature and high mineralization degree, which cannot meet the construction requirements and causes potential damage to the reservoir environment.

Method used

Using a preparation method of a suspended thickener for fracturing, an internal phase dispersible polymer is prepared by aqueous solution radical polymerization reaction, and combined with an external phase organic alcohol and a dispersant additive to form an efficient suspension thickener. Including acrylamide, 2-acrylamide-2-methylpropanesulfonic acid and N-vinylpyrrolidone, clay stabilizer and polyvinyl butyral are added to improve the dispersion and temperature resistance of the polymer.

Benefits of technology

It achieves good suspension performance and shear resistance in high-temperature deep wells, reduces construction costs, improves the recycling rate of the rubber breaking liquid and protects the reservoir, and meets the construction needs of different reservoirs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879299A_ABST
    Figure CN118879299A_ABST
Patent Text Reader

Abstract

The invention relates to a suspension thickening agent for fracturing and a preparation method thereof. The method comprises the following steps: taking a polyacrylamide terpolymer (AM / AMPS / NVP) prepared from acrylamide, 2-acrylamido-2-methylpropanesulfonic acid and N-vinyl pyrrolidone through an aqueous solution free radical polymerization reaction as an internal phase dispersoid; a blended solution of low-molecular alcohol, a dispersing agent auxiliary agent and an alcohol-soluble thickening agent is used as an external-phase dispersing agent; the internal phase dispersoid and the external phase dispersing agent are fully stirred and mixed to obtain the suspension thickening agent for fracturing. The prepared suspension thickening agent for fracturing can be used as a slickwater fracturing fluid, and has the characteristics of low friction resistance and excellent salt resistance; and the fracturing fluid can also be used as a high-temperature-resistant fracturing fluid, can be safely and effectively applied in a high-temperature deep well at 150 DEG C, and has excellent temperature resistance and shear resistance. Meanwhile, flowback and recycling of the gel breaking fluid can be achieved, the construction cost is effectively reduced, the damage degree to the reservoir environment is low, and the gel breaking fluid can be used as a clean fracturing fluid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of oil and gas field exploitation, and in particular relates to a suspension thickener for fracturing and a preparation method thereof. Background Art

[0002] Hydraulic fracturing is one of the most important measures to increase production in my country's oil and gas field exploitation. The performance of fracturing fluid is directly related to the construction effect. Slickwater fracturing fluid is widely used in the development of shale oil and gas reservoirs due to its high efficiency and low cost. High temperature resistant fracturing fluid has attracted much attention as the focus of oil exploration shifts to deep reservoirs. In recent years, my country's oil and gas field reservoirs have shown a trend of complexity, which has put forward higher requirements on the performance of fracturing fluid.

[0003] Fracturing fluids include powder and suspension. Among them, polyacrylamide polymer powder thickeners have the following problems: 1. It is easy to form dust pollution during fracturing construction, and the polymer powder has poor solubility and is easy to form "fish-eye" insoluble matter; 2. It cannot be mixed and injected continuously, and the construction needs to prepare the liquid in advance, which affects the construction efficiency. The problems with the currently commonly used suspended thickeners are: 1. For the currently exploited deep wells, high-temperature, and high-mineralization unconventional oil reservoirs, the temperature and salt resistance of conventional suspended thickeners are insufficient, and the fracturing fluid is prone to "sanding" when injected into the formation, affecting construction safety and mining efficiency; 2. The resistance reduction performance of conventional suspended thickeners is relatively low. During the fracturing process, the friction between the fracturing fluid and the pipeline, rock wall, cracks, etc. will cause a large load on the high-pressure pump group on the ground, which can easily cause excessive underground pressure and affect both construction results and costs; 3. After the fracturing fluid configured with conventional suspended thickeners breaks the gel in the formation, the surface interfacial tension of the broken gel fluid is relatively large, which increases the difficulty of returning the broken gel fluid for reuse. At the same time, the broken gel fluid has a high residue content, which causes great damage to the reservoir environment.

[0004] The document with application number "202011432107.5" discloses "a high-efficiency salt-resistant dual-purpose thickener and its preparation method and application". The preparation method of the thickener includes S1 preparation of water phase; S2 preparation of oil phase; S3 emulsification; S4 polymerization; S5 post-treatment. Hydrophobic monomers, functional monomers and salt-resistant monomers are introduced into the thickener to form a dense and complex spatial network structure in the aqueous solution. The problems with this technical solution are: 1. The preparation process of the emulsion is complicated and the cost of raw materials is high; 2. The emulsion-type thickener has good heat and shear resistance at 90°C, but it has not been tested at higher temperatures, and it is not certain whether it can be used safely in ultra-high temperature deep wells; 3. The performance of the fracturing fluid degelling fluid has not been tested, and the feasibility of the return and reuse of the degelling fluid and the degree of damage to the reservoir environment are unknown. Summary of the invention

[0005] The invention provides a method for preparing a suspension thickener for fracturing, so as to solve the problems in the prior art of complex preparation process, high raw material cost, difficulty in meeting construction requirements in deep well high temperature and high mineralization unconventional oil reservoirs, and possible damage to the reservoir environment.

[0006] In order to achieve the above object, the specific scheme of the present invention is as follows: a method for preparing a suspension thickener for fracturing, characterized in that: it comprises the following components in parts by weight: 30 parts of an internal phase dispersed polymer, 20-40 parts of an external phase organic alcohol mixed solvent, 20-40 parts of an alcohol-soluble thickener, and 5-10 parts of a dispersant aid;

[0007] The specific preparation steps are as follows:

[0008] Step 1: Prepare ingredients:

[0009] Preparation of internal phase dispersed polymer: acrylamide (AM), 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and N-vinylpyrrolidone (NVP) were prepared by aqueous solution free radical polymerization to obtain polyacrylamide-based terpolymer (AM / AMPS / NVP);

[0010] Preparation of an external phase organic alcohol mixed solvent: Mixing a plurality of organic alcohol reagents and stirring to obtain a mixed solvent;

[0011] Step 2: Add the dispersant additive to the external phase organic alcohol mixed solvent, and continue stirring for 5-10 minutes to obtain a mixed alcohol solvent;

[0012] Step 3: adding an alcohol-soluble thickener to the mixed alcohol solvent, stirring at a speed of 6000-8000 r / min for 5-10 min to obtain an external phase dispersant;

[0013] Step 4: Mix the external phase dispersant and the internal phase dispersoid polymer, and stir at a high speed of 8000-9000 r / min for 10-15 minutes to obtain a suspension thickener for fracturing.

[0014] Furthermore, the above-mentioned multiple organic alcohol reagents are isopropanol, methanol and ethylene glycol in a mass ratio of 4-7:2-4:1-2.

[0015] Furthermore, the above-mentioned dispersant auxiliary agent is one of OP-10 and sodium lauryl sulfate.

[0016] Furthermore, the alcohol-soluble thickener is a mixture of a clay stabilizer and polyvinyl butyral or polyethylene glycol 10000, and the mass ratio of polyvinyl butyral or polyethylene glycol 10000 to the clay stabilizer is 1:0.6-4.

[0017] Furthermore, the clay stabilizer is alcohol-based bentonite initiated by white oil, and the mass ratio of alcohol-based bentonite to white oil is 1:2 to prepare the clay stabilizer.

[0018] Furthermore, the suspension thickener for fracturing is prepared by the above preparation method.

[0019] Compared with the prior art, the present invention has the following advantages:

[0020] 1. Since the alcohol-soluble thickener added to the external phase dispersant is a mixture of clay stabilizer and polyvinyl butyral or polyethylene glycol 10000, it can effectively increase the viscosity of the low molecular alcohol solvent, which is beneficial to improve the suspension ability of the polymer in the dispersant, and there will be no "sedimentation" of the polymer. The experimental results show that within 30 days, the suspension performance of the suspension thickener for fracturing is good.

[0021] 2. One product has three uses: Due to the addition of ethylene glycol and dispersant additive OP-10 to the polymer, the polymer is better dispersed in the solvent, the dissolution rate is faster, and the dissolution performance is better.

[0022] The suspension thickener for fracturing can be used as a slick water fracturing fluid. When the amount added is less than 0.05% to 0.4%, the drag reduction rate of the solution is greater than 70%. According to the NBT14003.3-2017 standard, the performance index of the product of the present invention as a slick water fracturing fluid meets the requirements of on-site construction, and has the characteristics of low friction and salt resistance. When the amount added is large, it can be used as a high temperature resistant fracturing fluid with high apparent viscosity, excellent heat resistance and shear resistance, and is suitable for high temperature deep well operations.

[0023] The product of the present invention can achieve seamless switching between low-viscosity slippery water fracturing fluid and high-viscosity high-temperature resistant fracturing fluid by adjusting the added amount, and can be effectively and safely used in ultra-high temperature deep wells at 150°C. The surface interfacial tension of the fracturing fluid degelling liquid is low, and the degelling liquid can be returned and reused, which can effectively reduce the construction cost. The degelling liquid has a low residue content and a low degree of damage to the reservoir environment, and can be used as a clean fracturing fluid. It can be used in different fracturing construction sites, is easy to operate, can effectively improve construction efficiency, and has broad application prospects in large-scale fracturing sites.

[0024] 3. Since the polymer molecular chain in the internal phase dispersed substance of the present invention contains 2-acrylamide-2-methylpropanesulfonic acid macromolecular groups, it is beneficial to improve the rigidity of the polymer molecular chain; at the same time, due to the introduction of -SO 3 H group and temperature-resistant monomer N-vinyl pyrrolidone, the salt resistance and temperature resistance of the polymer are improved. When the suspension thickener for fracturing is used as a high-temperature resistant fracturing fluid, 0.8% thickener, deionized water solution and 1.0% thickener, 5% standard salt water solution, 150℃, 170s -1At the shear rate, the residual shear viscosity after shearing for 1 hour is 50.87mPa·s and 50.26mPa·s respectively. The viscosity after shearing is greater than 50mPa·s of the SYT 6376-2008 general technical conditions standard for fracturing fluid, indicating that the suspension thickener for fracturing has good temperature and shear resistance and meets the requirements of on-site construction.

[0025] 4. The types of raw materials added to the external phase dispersant are relatively small, the additives are safe, non-toxic and inexpensive; the preparation process of the suspension thickener for fracturing is simple and the cost is low, which can achieve the goal of reducing costs and increasing efficiency.

[0026] 5. The product has a wide range of applications: For shale gas reservoirs, the product of the present invention is used as a low-viscosity slickwater fracturing fluid, and the prepared thickener needs to have good drag reduction ability; for reservoirs with high temperatures, the prepared thickener has good temperature resistance and can be used as a high-viscosity high-temperature resistant fracturing fluid. Therefore, the product prepared by the present invention has a wide range of applications for shale gas reservoirs, medium and low reservoirs, and deep well reservoirs with higher temperatures. It can be applied to reservoirs with different characteristics, can meet most construction requirements, and is of great significance for promoting oil and gas field exploitation. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The stability performance test of the thickener prepared in Example 3;

[0028] Figure 2 This is a test diagram of the drag reduction performance of the thickener prepared in Example 3;

[0029] Figure 3 This is a test chart of the heat and shear resistance of the thickener prepared in Example 3 at 90°C;

[0030] Figure 4 This is a test chart of the heat and shear resistance of the thickener prepared in Example 3 at 150°C. DETAILED DESCRIPTION

[0031] The present invention will be further described in detail below in conjunction with specific examples, but the implementation methods of the present invention include but are not limited to the scope represented by the following examples.

[0032] Embodiment 1, a method for preparing a suspension thickener for fracturing, comprising the following steps:

[0033] Step 1: Prepare the materials, all parts are by weight:

[0034] Preparation of internal phase dispersed polymer: acrylamide (AM), 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and N-vinylpyrrolidone (NVP) in a mass ratio of 6:2:1 were prepared by aqueous solution free radical polymerization to obtain polyacrylamide-based terpolymer (AM / AMPS / NVP);

[0035] Prepare the external phase organic alcohol mixed solvent: add 14 parts of isopropanol, 4 parts of methanol and 2 parts of ethylene glycol into a beaker respectively, and stir magnetically until the external phase organic alcohol mixed solvent is completely mixed and uniform;

[0036] Step 2: Dissolve 5 parts of dispersant aid OP-10 in 20 parts of external organic alcohol mixed solvent under magnetic stirring for 5 minutes to obtain a mixed alcohol solvent;

[0037] Step 3, adding 20 parts of an alcohol-soluble thickener to a mixed alcohol solvent, wherein the alcohol-soluble thickener is 4 parts of polyvinyl butyral and 16 parts of a clay stabilizer, wherein the clay stabilizer is an alcohol-based bentonite initiated by white oil, and the mass ratio of the alcohol-based bentonite to the white oil is 1:2; stirring at a constant speed mixer at a speed of 6000r / min for 5 minutes, so that the polyvinyl butyral is completely dissolved in the mixed alcohol solvent, and the clay stabilizer is evenly dispersed in the mixed alcohol solvent, to prepare an external phase dispersant;

[0038] Step 4: Take 30 parts of the endogenous dispersoid polymer and add it to the external phase dispersant prepared in step 3, stir it at a high speed of 8000 r / min in a constant speed mixer for 10 minutes to prepare a suspension thickener product for fracturing.

[0039] Embodiment 2, a method for preparing a suspension thickener for fracturing, comprising the following steps:

[0040] Step 1: Prepare the materials, all parts are by weight:

[0041] Preparation of internal phase dispersed polymer: acrylamide (AM), 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and N-vinylpyrrolidone (NVP) in a mass ratio of 6:2:1 were prepared by aqueous solution free radical polymerization to obtain polyacrylamide-based terpolymer (AM / AMPS / NVP);

[0042] Preparation of an external phase organic alcohol mixed solvent: 21 parts of isopropanol, 6 parts of methanol, and 3 parts of ethylene glycol are added into a beaker respectively, and magnetic stirring is performed until the external phase organic alcohol mixed solvent is completely mixed and uniform;

[0043] Step 2: Dissolve 10 parts of dispersant aid OP-10 in 30 parts of external organic alcohol mixed solvent by magnetic stirring for 5 minutes to obtain a mixed alcohol solvent;

[0044] Step 3, adding 30 parts of an alcohol-soluble thickener to a mixed alcohol solvent, wherein the alcohol-soluble thickener is 6 parts of polyethylene glycol 10000 and 24 parts of a clay stabilizer, wherein the clay stabilizer is an alcohol-based bentonite initiated by white oil, and the mass ratio of the alcohol-based bentonite to the white oil is 1:2; completely dissolving the mixture in the mixed alcohol solvent under magnetic stirring to prepare an external phase dispersant;

[0045] Step 4: Take 30 parts of the endogenous dispersoid polymer and add it to the external phase dispersant prepared in step 3, stir it at a high speed of 8000 r / min in a constant speed mixer for 10 minutes to prepare a suspension thickener product for fracturing.

[0046] Embodiment 3, a method for preparing a suspension thickener for fracturing, comprising the following steps:

[0047] Step 1: Prepare the materials, all parts are by weight:

[0048] Preparation of internal phase dispersed polymer: acrylamide (AM), 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and N-vinylpyrrolidone (NVP) in a mass ratio of 6:2:1 were prepared by aqueous solution free radical polymerization to obtain polyacrylamide-based terpolymer (AM / AMPS / NVP);

[0049] Prepare an organic alcohol solvent: add 28 parts of isopropanol, 8 parts of methanol, and 4 parts of ethylene glycol into a beaker, respectively, and stir magnetically until the organic alcohol mixed solvent is completely mixed and uniform;

[0050] Step 2: Dissolve 10 parts of dispersant additive OP-10 in 40 parts of organic alcohol solvent under magnetic stirring for 5 minutes to obtain a mixed alcohol solvent;

[0051] Step 3, adding 40 parts of an alcohol-soluble thickener to a mixed alcohol solvent, wherein the alcohol-soluble thickener is 8 parts of polyvinyl butyral and 32 parts of a clay stabilizer, wherein the clay stabilizer is an alcohol-based bentonite initiated by white oil, and the mass ratio of the alcohol-based bentonite to the white oil is 1:2; stirring at a constant speed mixer at a speed of 6000r / min for 5 minutes, so that the polyvinyl butyral is completely dissolved in the mixed alcohol solvent, and the clay stabilizer is evenly dispersed in the mixed alcohol solvent, to prepare an external phase dispersant;

[0052] Step 4: Add 30 parts of the endogenous dispersoid polymer to the external phase dispersant prepared in step 3, and stir at high speed for 10 minutes at a speed of 8000 r / min in a constant speed mixer to prepare a suspension thickener product for fracturing.

[0053] Embodiment 4, a method for preparing a suspension thickener for fracturing, comprising the following steps:

[0054] Step 1: Prepare the materials, all parts are by weight:

[0055] Preparation of internal phase dispersed polymer: acrylamide (AM), 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and N-vinylpyrrolidone (NVP) in a mass ratio of 6:2:1 were prepared by aqueous solution free radical polymerization to obtain polyacrylamide-based terpolymer (AM / AMPS / NVP);

[0056] Preparation of an external phase organic alcohol mixed solvent: 21 parts of isopropanol, 12 parts of methanol, and 6 parts of ethylene glycol are added into a beaker respectively, and magnetic stirring is performed until the external phase organic alcohol mixed solvent is completely mixed and uniform;

[0057] Step 2: dissolving 8 parts of dispersant aid sodium dodecyl sulfate in 39 parts of organic alcohol solvent under magnetic stirring for 10 minutes to obtain a mixed alcohol solvent;

[0058] Step 3, adding 30 parts of an alcohol-soluble thickener to a mixed alcohol solvent, wherein the alcohol-soluble thickener is 12 parts of polyethylene glycol 10000 and 18 parts of a clay stabilizer, wherein the clay stabilizer is an alcohol-based bentonite initiated by white oil, and the mass ratio of the alcohol-based bentonite to the white oil is 1:2; stirring at a constant speed mixer at a speed of 6000r / min for 5 minutes, so that the polyethylene glycol 10000 is completely dissolved in the mixed alcohol solvent, and the clay stabilizer is evenly dispersed in the mixed alcohol solvent, to prepare an external phase dispersant;

[0059] Step 4: Add 30 parts of the endogenous dispersoid polymer to the external phase dispersant prepared in step 3, and stir at high speed for 15 minutes at a speed of 8000 r / min in a constant speed mixer to prepare a suspension thickener product for fracturing.

[0060] Embodiment 5, a method for preparing a suspension thickener for fracturing, comprising the following steps:

[0061] Step 1: Prepare the materials, all parts are by weight:

[0062] Preparation of internal phase dispersed polymer: acrylamide (AM), 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and N-vinylpyrrolidone (NVP) in a mass ratio of 6:2:1 were prepared by aqueous solution free radical polymerization to obtain polyacrylamide-based terpolymer (AM / AMPS / NVP);

[0063] Prepare the external phase organic alcohol mixed solvent: add 12 parts of isopropanol, 12 parts of methanol and 6 parts of ethylene glycol into a beaker respectively, and stir magnetically until the external phase organic alcohol mixed solvent is completely mixed and uniform;

[0064] Step 2: Dissolve 5 parts of dispersant aid sodium dodecyl sulfate in 30 parts of organic alcohol solvent under magnetic stirring for 5 minutes to obtain a mixed alcohol solvent;

[0065] Step 3: Add 20 parts of an alcohol-soluble thickener to a mixed alcohol solvent, wherein the alcohol-soluble thickener is 12 parts of polyvinyl butyral and 8 parts of a clay stabilizer, wherein the clay stabilizer is an alcohol-based bentonite initiated by white oil, and the mass ratio of the alcohol-based bentonite to the white oil is 1:2; stir at a high speed of 6000 r / min in a constant speed mixer for 10 minutes, so that the polyvinyl butyral and polyethylene glycol 10000 are completely dissolved in the mixed alcohol solvent, and the clay stabilizer is evenly dispersed in the mixed alcohol solvent to prepare an external phase dispersant;

[0066] Step 4: Add 30 parts of the endogenous dispersoid polymer to the external phase dispersant prepared in step 3, stir at a high speed of 9000 r / min in a constant speed mixer for 10 minutes to prepare a suspension thickener product for fracturing.

[0067] Performance Test:

[0068] 1. Stability performance test

[0069] The prepared suspension thickener for fracturing was placed at room temperature to test its bulk viscosity and observe the suspension stability of the polymer in the external phase dispersant (see Figure 1 ). The test results are shown in Table 1.

[0070] Table 1 Stability performance test

[0071]

[0072] As can be seen from Table 1, the viscosity and stability of the suspension thickener for fracturing prepared in the embodiment meet the construction requirements. The appropriate viscosity and good stability facilitate the storage of the suspension thickener after preparation and its subsequent field application.

[0073] 2. Solubility and thickening performance test

[0074] The suspension thickener prepared in the example was respectively prepared into 0.8% fracturing fluid in deionized water, and the apparent viscosity of the solution was measured using a six-speed rotary viscometer and the time required to reach the maximum viscosity was recorded. The test results are shown in Table 2.

[0075] Table 2 Dissolution and thickening performance test

[0076]

[0077] As can be seen from Table 2, the suspension thickener prepared in Example 3 has a shorter dissolution time and a higher final viscosity at the same mass fraction, indicating that it has good thickening ability and meets the on-site continuous mixing and injection process.

[0078] Taking Example 3 as the best example, the suspension thickener prepared in Example 3 was then tested for drag reduction performance and heat and shear resistance.

[0079] 3. Drag reduction performance test

[0080] The suspension thickener prepared in Example 3 was respectively prepared into slick water fracturing fluids with addition amounts of 0.05%, 0.1%, 0.2%, 0.3% and 0.4% with deionized water, 10% standard brine, 30% standard brine and 50% standard brine, and the drag reduction performance was tested using a friction tester. Figure 2 The test results show that when this fracturing suspension thickener is used as a slick water fracturing fluid, the drag reduction rate is greater than 70%, with excellent drag reduction effect, performance indicators exceeding the NBT14003.3-2017 standard, and meeting the requirements of on-site construction. When the addition amount is 0.1%, the drag reduction performance is the best.

[0081] 4. Temperature and shear resistance test

[0082] The heat and shear resistance of the suspension thickener for fracturing prepared in Example 3 was tested using a HAAKE MARS IV rheometer. 0.8% and 1.0% suspension thickener solutions were prepared in deionized water and 5% standard saline, respectively.

[0083] Shear resistance test was carried out at 90°C with a shear rate of 170s -1 , heated to 90℃ and sheared for 1h. The results are as follows Figure 3 As shown in Figure 2, at 90°C, the residual shear viscosities of the two fracturing fluids after shearing for 1 h were 78.02 mPa·s (see Figure 3 -a) and 76.33 mPa·s (see Figure 3 -b).

[0084] Shear resistance test was carried out at 150°C with a shear rate of 170s. -1 , heating to 150℃ and shearing for 1h, the results are as follows Figure 4 As shown in Figure 2, at 150°C, the residual shear viscosities of the two fracturing fluids after shearing for 1 h were 50.87 mPa·s (see Figure 4 -a) and 50.26 mPa·s (see Figure 4 -b).

[0085] This shows that the suspension thickener for fracturing has excellent heat and shear resistance and is suitable for high-temperature deep well fracturing operations.

[0086] 5. Gel breaking liquid performance test

[0087] The lower the apparent viscosity, surface tension and interfacial tension of the fracturing fluid, the easier it is to recycle and reuse the fracturing fluid; the less residue the fracturing fluid contains, the less damage it will cause to the reservoir. 4 ) 2 S 2 O 8 Experiments were conducted for the gel breakers.

[0088] The fracturing suspension thickener prepared in Example 3 was tested for its performance as a fracturing fluid debonding fluid. 0.8% and 1.0% suspension thickener solutions were prepared in deionized water and 5% standard saline, respectively. 0.04% (NH 4 ) 2 S 2 O 8 The gel was broken at 50, 60 and 70°C, and the performance of the gel-breaking liquid was tested. The results are shown in Tables 3 and 4.

[0089] Table 3 Degelling performance test of suspension thickener solution with a mass fraction of 0.8%

[0090]

[0091] Table 4 Performance test of 1.0% mass fraction suspension thickener and 5% standard saline degelling liquid

[0092]

[0093] As shown in Tables 3 and 4, the deionized water solution of 0.8% suspension thickener by mass, the suspension thickener by mass, and the 5% standard saline solution by mass, with the addition of 0.04% ammonium persulfate (APS) at 50, 60, and 70°C, can completely break the gel within the specified release time. The surface tension and interfacial tension of the broken gel liquid are both lower than 28mN / m and 2mN / m. The viscosity of the broken gel liquid is less than 5mPa·s. The residue content of the broken gel liquid is less than 22mg / L. The suspension thickener solution has good breaking performance and backflow capacity, and relatively little pollution to the reservoir.

[0094] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may be modified and varied in various forms. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a suspension thickener for fracturing, Features: The invention comprises the following components in parts by weight: 30 parts of an inner phase dispersoid polymer, 20-40 parts of an outer phase organic alcohol mixed solvent, 20-40 parts of an alcohol-soluble thickener, and 5-10 parts of a dispersant auxiliary; The specific preparation steps are as follows: Step 1: Prepare ingredients: Preparation of internal phase dispersed polymers: acrylamide (AM), 2-acrylamido-2-methylpropanesulfonic acid (AMPS) and N - Polyacrylamide-based terpolymers (AM / AMPS / NVP) were prepared by free radical polymerization of vinyl pyrrolidone (NVP) in aqueous solution; Preparation of an external phase organic alcohol mixed solvent: Mixing a plurality of organic alcohol reagents and stirring to obtain a mixed solvent; Step 2: Add the dispersant additive to the external phase organic alcohol mixed solvent, and continue stirring for 5-10 minutes to obtain a mixed alcohol solvent; Step 3, adding an alcohol-soluble thickener to the mixed alcohol solvent, stirring at a speed of 6000-8000 r / min for 5-10 min to obtain an external phase dispersant; Step 4: Mix the external phase dispersant and the internal phase dispersoid polymer, and stir at a high speed of 8000-9000 r / min for 10-15 min to obtain a suspension thickener for fracturing.

2. The method for preparing the suspension thickener for fracturing according to claim 1, Features: The multiple organic alcohol reagents are isopropanol, methanol and ethylene glycol in a mass ratio of 4-7:2-4:1-2.

3. The method for preparing the suspension thickener for fracturing according to claim 1, Features: The dispersant auxiliary agent is one of OP-10 and sodium lauryl sulfate.

4. The method for preparing the suspension thickener for fracturing according to claim 1, Features: The alcohol-soluble thickener is a mixture of a clay stabilizer and polyvinyl butyral or polyethylene glycol 10000, and the mass ratio of the clay stabilizer to polyvinyl butyral or polyethylene glycol 10000 is 1:0.6-4.

5. The method for preparing the suspension thickener for fracturing according to claim 4, Features: The clay stabilizer is alcohol-based bentonite initiated by white oil, and the mass ratio of alcohol-based bentonite to white oil is 1:2 to prepare the clay stabilizer.

6. The suspension thickener for fracturing obtained by the preparation method according to claim 1.

Citation Information

Patent Citations

  • Temperature resistant water base fracturing fluid thickening agent and preparation thereof

    CN101475797A

  • High-temperature-resistant full-suspension low-damage fracturing fluid and preparation method thereof

    CN109652053A

  • Anti-water-locking easily-dissolved alcohol-based fracturing fluid and preparation method thereof

    CN113150766A

  • Thickening agent suspension emulsion for fracturing fluid and preparation method thereof

    CN113355079A

  • Water-soluble concentrated thickening agent for fracturing and preparation method thereof

    CN116925728A

Cited By

  • Polyacrylamide emulsion based on alcohol-based dispersion liquid and preparation method thereof

    CN119955503A

  • An acrylamide emulsion based on an alcohol-based dispersion liquid and a preparation method thereof