Eu < 3 + >-doped ZnO hierarchical nanostructure and preparation method thereof

Preparation of Eu3+ doped ZnO graded nanostructures by plasma arc method, solving the problems of low purity and high cost in the prior art, realizing high purity and low cost nanostructure preparation, with strong red light and photocatalytic properties, suitable for in optoelectronic devices.

CN118879310AActive Publication Date: 2024-11-01BOHAI UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410904768.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-01
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

In the prior art, the preparation of Eu3+ doped ZnO graded nanostructures has low purity and high cost, and is difficult to achieve nanostructures with high yield, uniform scale, controllable doping, good monochromaticity and high luminescence intensity.

Method used

After mixing Zn powder and Eu2O3 powder in proportion by plasma arc method, react in a graphite pot through a DC arc discharge device, and use circulating cooling water and air environment to generate Eu3+ doped ZnO graded nanostructures, and the nanostructures are made of nanoparticles. It is composed of a number of nanoneedles, with a diameter of 300-500 nm and a length of 100-300 nm, and has strong red light and photocatalytic properties.

Benefits of technology

The preparation of Eu3+ doped ZnO graded nanostructures with high purity, low cost and easy to operate is achieved, with strong red light and photocatalytic properties, suitable for industrial production, and suitable for micro-nano devices and optoelectronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879310A_ABST
    Figure CN118879310A_ABST
Patent Text Reader

Abstract

The invention discloses an Eu < 3 + >-doped ZnO graded nanostructure and a preparation method thereof, and the specific method comprises the following steps: uniformly mixing Zn powder and Eu2O3 powder in proportion, and pressing into a mixed powder briquette; putting the briquette into a graphite pot, and putting the graphite pot into a copper pot anode in a reaction chamber of a direct-current arc discharge device; the tungsten rod cathode and the copper pot anode are oppositely and vertically arranged; introducing air into the reaction chamber, and introducing circulating cooling water into the copper pot; and operating the discharge reaction. The preparation method is simple in condition, easy to operate, efficient, energy-saving and environment-friendly, no harmful gas is generated in the process, the Eu < 3 + >-doped ZnO graded nanostructure prepared through the method is uniform in structure, high in purity and strong in red light and photocatalytic performance, and infinite possibility is provided for micro-nano devices and photoelectric devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of LED fluorescent powder and nano material preparation, and particularly relates to a simple method for preparing Eu 3+ A new approach to doping ZnO hierarchical nanostructures. Background Art

[0002] ZnO is an important semiconductor material with important applications in electronics, optoelectronics, optics, sensors and other fields. Its unique photoelectric properties, chemical stability and biocompatibility make it a hot spot for research and application. By carefully introducing luminescent centers such as transition metal ions or rare earth metal ions, the emission characteristics of ZnO semiconductors can be precisely controlled to optimize emission bands at specific wavelengths. This breakthrough adjustment is of great significance for realizing a wide range of application scenarios, including multicolor emission of light-emitting devices, and shows broad research value and application potential. Among the many rare earth ions, Eu 3+ It has attracted widespread attention due to its strong red emission characteristics in the 610-620nm range. However, due to the huge differences in ionic radius and charge, it is still very challenging to dope Eu3+ into ZnO.

[0003] Several synthetic methods, such as chemical bath deposition, hydrothermal, electrodeposition, combustion, and coprecipitation, have been reported to control the particle size in the nanoscale range and develop red-luminescent Eu 3+ Doped ZnO nanomaterials have special nanostructures such as nanowires, nanoflowers, nanorods, nanopillars, nanobelts and ellipses. The above preparation and deposition methods require long-term heating, metal catalysts and substrates, which greatly increases the preparation cost. In addition, the chemical method for preparing Eu 3+ Doping ZnO nanomaterials takes a long time and has low yields, and cannot effectively avoid the introduction of impurity elements. In addition, the synthesis of complex three-dimensional (3D) ZnO nanostructures, especially 3D nanostructures composed of one-dimensional nanostructures, has attracted widespread attention.

[0004] Therefore, it is urgent to find a method that is simple in process, low in cost, suitable for industrial production, and can prepare Eu with high purity, high yield, uniform size, controllable doping, good monochromaticity and high luminescence intensity. 3+ A new method for doping ZnO with new nanostructures. In order to solve the above problems, this patented technology is dedicated to preparing Eu by plasma arc method. 3+ Doped ZnO hierarchical nanostructures. Summary of the invention

[0005] The object of the present invention is to provide a Eu 3+ Doped ZnO hierarchical nanostructure and its preparation method solve the problem of preparing Eu 3+The technical problems of low purity and high cost of doped ZnO graded nanostructures. The preferred technical solutions among the many technical solutions provided by the present invention can produce many technical effects as described below.

[0006] To achieve the above object, the present invention provides the following technical solutions: a Eu 3+ The hierarchical nanostructure doped with ZnO is composed of nanoparticles and a plurality of nanoneedles radiating outward from the nanoparticles as the center, the overall diameter of the hierarchical nanostructure is 300-500nm, the length of the nanoneedles is 100-300nm, and the diameter is 10-20nm. The hierarchical structure has strong red light and photocatalytic properties.

[0007] The present invention also provides a Eu 3+ The preparation method of doped ZnO hierarchical nanostructure comprises the steps of: mixing Zn powder and Eu 2 O 3 The powders are mixed evenly according to the proportion and pressed into mixed powder briquettes; the briquettes are placed in a graphite pot and then placed in a copper pot anode in the reaction chamber of a DC arc discharge device; the tungsten rod cathode and the copper pot anode are placed vertically relative to each other; the reaction chamber is filled with air and circulating cooling water is passed into the copper pot; the discharge reaction is operated; the grayish yellow fluffy powder collected on the condensation wall is Eu 3+ Doped ZnO hierarchical nanostructure.

[0008] Furthermore, in the method, Zn powder and Eu 2 O 3 The powder mixing molar ratio is 100:1-2.

[0009] Furthermore, the air pressure in the reactor is 20-40 kPa.

[0010] Furthermore, in the method, the reaction voltage is 20 to 30 V, the current is 60 to 80 A, and the reaction time is 10 to 30 seconds.

[0011] Compared with the prior art, the preferred embodiment of the present invention provides Eu 3+ The preparation method of doped ZnO hierarchical nanostructures has simple conditions, is easy to operate, is highly efficient and energy-saving, and is environmentally friendly, and no harmful gases are generated during the process. 3+ The uniform and high purity doped ZnO hierarchical nanostructure has strong red light and photocatalytic properties, providing unlimited possibilities for micro-nano devices and optoelectronic devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below, but the scope of protection claimed by the present invention is not limited to the scope described in the embodiments.

[0013] Figure 1 It is a schematic diagram of the structure of the reaction device used in the method of the present invention;

[0014] Figure 2 Eu prepared in Example 1 of the present invention 3+ SEM image of doped ZnO hierarchical nanostructure;

[0015] Figure 3 Eu prepared in Example 1 of the present invention 3+ SEM image of doped ZnO hierarchical nanostructure;

[0016] Figure 4 Eu prepared in Example 1 of the present invention 3+ XRD pattern of doped ZnO hierarchical nanostructures;

[0017] Figure 5 Eu prepared in Example 1 of the present invention 3+ EDS spectrum of doped ZnO hierarchical nanostructures;

[0018] Figure 6 Eu prepared in Example 1 of the present invention 3+ Excitation spectrum of ZnO-doped hierarchical nanostructures (emission at 611 nm);

[0019] Figure 7 Eu prepared in Example 1 of the present invention 3+ Emission spectrum of doped ZnO hierarchical nanostructures (under 467nm excitation);

[0020] Figure 8 Eu prepared in Example 1 of the present invention 3+ UV-Vis absorption spectra of photocatalytic degradation of methyl orange over time by ZnO-doped hierarchical nanostructures

[0021] Fig. 9 Eu prepared in Example 2 of the present invention 3+ SEM image of doped ZnO hierarchical nanostructure;

[0022] Fig.10 Eu prepared in Example 2 of the present invention 3+ SEM image of doped ZnO hierarchical nanostructure;

[0023] Fig.11 is a SEM image of undoped ZnO nanowires prepared in Example 3 of the present invention;

[0024] Fig.12 is the emission spectrum of the undoped ZnO nanowires prepared in Example 3 of the present invention (under 325nm excitation);

[0025] Fig.13 The UV-visible absorption spectrum of the photocatalytic degradation of methyl orange by undoped ZnO nanowires prepared in Example 3 of the present invention varies with time.

[0026] Figure 1 In the figure: 1. Reaction chamber; 2. Condensation wall; 3. Tungsten cathode; 4. Reaction raw materials; 5. Graphite crucible anode; 6. Copper seat (including water inlet and outlet); 7. Air inlet; 8. Air outlet; 9. Condensation wall water inlet; 10. Condensation wall water outlet. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention.

[0028] Figure 1 It is a schematic diagram of the structure of the DC arc system used in the method of the present invention.

[0029] like Figure 1 As shown, the reaction chamber 1 is provided with a condensation wall 2, a tungsten cathode 3 and a graphite crucible anode 5, wherein the graphite crucible anode 5 is filled with reaction raw materials 4 (Zn powder and Eu 2 O 3 The graphite crucible anode 5 and the tungsten cathode 3 are connected to a DC power supply. In order to ensure the rapid growth of the nanowires, circulating cooling water is provided at the graphite crucible anode 5 and the condensation wall 2, wherein a cooling water inlet and outlet are provided below the graphite crucible anode 5, that is, Figure 1 The cooling water inlet 6 (the cooling water inlet 6 includes a water inlet and a water outlet), and the two ends of the condensation wall 2 are respectively provided with a condensation wall water inlet 9 and a condensation wall water outlet 10. After the reaction is completed, the collected product is Eu 3+ Doped ZnO hierarchical nanostructures.

[0030] A condensation wall 2 is provided in the reaction chamber 1. Cooling water (the cooling water can be recycled) needs to be introduced into the graphite crucible anode 5 and the condensation wall 2 to reduce the temperature of the graphite crucible anode 5 and the condensation wall 2, so that a larger temperature gradient is generated in the reaction chamber, which is conducive to the rapid growth of the ZnO hierarchical nanostructure.

[0031] Example 1

[0032] In this example, Eu 3+ Doped ZnO hierarchical nanostructure, the material preparation process is as follows:

[0033] Metal Zn powder and Eu 2 O 3 The powder is fully mixed in a molar ratio of 100:1 and then put into a tableting mold to be pressed into a cylindrical ingot 4 with a height of 1-2 cm. The obtained ingot 4 is then placed in a graphite crucible 5 located in the reaction chamber of a DC arc discharge device, and the tungsten rod cathode 3 is fixed at a certain distance above the reaction raw material 4, while ensuring that the tip of the tungsten rod cathode 3 does not contact the reaction raw material 4; the reaction chamber 1 is evacuated to a vacuum and filled with 20 kPa of air as a reaction gas; the circulating water device is turned on, and cooling water is introduced from the condensation wall 2 and the copper seat 6; by adjusting the height of the copper seat 6, the graphite crucible 5 and the tungsten rod 3 are contacted and the arc is opened for discharge. During the discharge process, the voltage is maintained at 30 V, the current is 60 A, and the reaction time is 10 s. A large amount of yellow fluffy powder collected on the condensation wall is Eu 3+ Doped ZnO hierarchical nanostructures.

[0034] Figure 2 For Eu 3+ The overall SEM image of the doped ZnO hierarchical nanostructure shows that the entire sample is a nano-hierarchical structure, and the overall diameter of each hierarchical nano unit is 300-400nm. Figure 3 From the locally enlarged SEM image of the sample, it can be seen that the single hierarchical nanostructure has a nanorod or nanoparticle in the middle, and multiple nanoneedles radiate outward from the nanorod or nanoparticle, with a length of 100-200nm and a diameter of 10-20nm.

[0035] Figure 4 Figure 2 is the XRD pattern. The diffraction peaks all correspond to the ZnO wurtzite structure, indicating that the sample has high purity and no impurities are present. Figure 5 The EDS spectrum of the sample shows that the atomic ratio of Zn, O and Eu is 54.7:43.9:1.4, indicating that the ZnO hierarchical nanostructure contains Eu ions.

[0036] Figure 6 For Eu 3+ Excitation line spectrum of doped ZnO hierarchical nanostructure under 611nm luminescence peak detection. The 380nm excitation peak of the spectrum is the excitation band of ZnO itself, and the 394nm, 404nm, 467nm and 533nm absorption peaks correspond to Eu 3+ of 7 F 0 - 5 L 6 , 7 F 0 - 5 D 3 , 7 F 0 - 5 D 2and 7 F 0 - 5 D 1 Transition. Figure 7 For the Eu 3+ PL spectrum of doped ZnO nanomaterials under 467nm excitation. 3+ The doped ZnO luminescent material emits red light at 610nm under the excitation of 467nm. This sharp emission peak is due to the Eu 3+ of 5 D 0 - 7 F 2 The other peaks at 592, 650 and 707 nm correspond to Eu 3+ The transition 5 D 0 - 7 F 1 , 5 D 0 - 7 F 3 and 5 D 0 - 7 F 4 . From ZnO hierarchical nanostructures with Eu 3+ The characteristic emission peak also proves that Eu 3+ doped into the ZnO lattice.

[0037] The UV-visible absorption spectrum of the dye can directly reflect the Eu 3+ Photocatalytic ability of doped ZnO hierarchical nanostructure. Weigh 50mg Eu 3+ The doped ZnO hierarchical nanostructures were added to 50 mL of methyl orange aqueous solution with a mass concentration of 15 mg / L. The photoluminescence of methyl orange under simulated visible light was used to investigate the effect of methyl orange on Eu 3+ The photocatalytic performance of ZnO hierarchical nanostructures was studied. Figure 8 As shown in the figure, with the extension of illumination time, the mass concentration of methyl orange solution gradually decreased. When the photocatalytic degradation time was 25 min, the methyl orange in the solution was basically photocatalytically degraded. 3+ The ZnO-doped hierarchical nanostructures exhibited good photocatalytic activity towards methyl orange.

[0038] Example 2

[0039] In this example, Eu 3+ Doped ZnO hierarchical nanostructure, the material preparation process is as follows:

[0040] Metal Zn powder and Eu 2 O 3The powder is fully mixed according to the molar ratio of 100:2 and then put into a tableting mold to be pressed into a cylindrical ingot 4 with a height of 1-2 cm. The obtained ingot 4 is then placed in a graphite crucible 5 located in the reaction chamber of the DC arc discharge device, and the tungsten rod cathode 3 is fixed at a certain distance above the reaction raw material 4, while ensuring that the tip of the tungsten rod cathode 3 does not contact the reaction raw material 4; the reaction chamber 1 is evacuated to vacuum and filled with 40kPa air as a reaction gas; the circulating water device is turned on, and cooling water is introduced from the condensation wall 2 and the copper seat 6; by adjusting the height of the copper seat 6, the graphite crucible 5 and the tungsten rod 3 are contacted and the arc is pulled open for discharge. During the discharge process, the voltage is maintained at 20V, the current is 80A, and the reaction time is about 30s. A large amount of yellow plush powder collected on the condensation wall is Eu3+ doped ZnO hierarchical nanostructure.

[0041] Fig. 9 This is the overall SEM image of the prepared sample. It can be seen that its morphology is a hierarchical nanostructure with uniform size, and the diameter of each hierarchical nanounit is 400-500nm. Fig.10 From the locally enlarged SEM image of the sample, it can be seen that there is a nanoparticle in the middle of a single nanounit, on which grow multiple nanoneedles with a length of 200-300nm and a diameter of 10-20nm.

[0042] Example 3

[0043] In this embodiment, undoped ZnO nanowires were prepared, and the material preparation process was as follows:

[0044] The metal Zn powder is placed in a tableting mold and pressed into a cylindrical ingot 4 with a height of 1-2 cm. The obtained ingot 4 is then placed in a graphite crucible 5 located in the reaction chamber of the DC arc discharge device, and the tungsten rod cathode 3 is fixed at a certain distance above the reaction raw material 4, while ensuring that the tip of the tungsten rod cathode 3 does not contact the reaction raw material 4; the reaction chamber 1 is evacuated to vacuum and filled with 20kPa air as a reaction gas; the circulating water device is turned on, and cooling water is introduced from the condensation wall 2 and the copper seat 6; by adjusting the height of the copper seat 6, the graphite crucible 5 and the tungsten rod 3 are contacted and the arc is pulled open for discharge. During the discharge process, the voltage is maintained at 10-12V, the current is 70A, and the reaction time is about 30s. ZnO wires are collected in the anode graphite crucible.

[0045] Fig.11 The SEM image of undoped ZnO nanowires has a length of about 1-5 μm and a diameter of about 80-120 nm. Fig.12 This is the PL spectrum of ZnO nanowires under 325nm excitation. There is a strong emission peak at 384nm, corresponding to the band gap of ZnO, and a wider green emission peak at 506nm, which is attributed to the radial recombination of photogenerated holes and singly ionized oxygen vacancy electrons, oxygen gaps, various defects and other effects. Fig.13 The UV-visible absorption spectrum of ZnO nanowires photocatalytic degradation over time. As the illumination time increases, the mass concentration of methyl orange solution gradually decreases. When the photocatalytic degradation time is 60 minutes, the methyl orange in the solution has not been completely photocatalytically degraded. This shows that the Eu in Example 1 3+ The photocatalytic activity of doped ZnO hierarchical nanostructures is significantly improved compared with that of undoped ZnO nanowires.

[0046] The above examples show that Eu 3+ Doping is the key to preparing ZnO hierarchical nanostructures. Doping Eu3+ with a large ionic radius into ZnO will produce a large number of zinc vacancy defects, which will be conducive to the secondary nucleation of nanoneedles and form a multi-ZnO hierarchical nanostructure. 3+ Doping into ZnO not only changes the luminescent properties of ZnO, but also changes the nanostructure of ZnO preparation. The new hierarchical nanostructure has a higher specific surface area, which significantly enhances the photocatalytic performance.

[0047] The above is only a specific embodiment of the present invention, which is used to illustrate the technical solution of the present invention but not to limit it. Although the present invention is described in detail with reference to the above embodiments, it should be understood by those skilled in the art that the technical solution of the invention can be modified or replaced by equivalents without departing from the scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. Eu 3+ Doped ZnO hierarchical nanostructure, characterized in that The hierarchical nanostructure consists of nanoparticles and a plurality of nanoneedles radiating outward from the nanoparticles as the center. The overall diameter of the hierarchical nanostructure is 300-500nm, and the nanoneedles are 100-300nm long and 10-20nm in diameter.

2. Eu 3+ The method for preparing a doped ZnO hierarchical nanostructure is characterized in that: The invention comprises the following steps: mixing Zn powder and Eu2O3 powder evenly according to a certain proportion, and pressing the mixed powder into a compact; placing the compact in a graphite pot, and placing the compact in a copper pot anode in a reaction chamber of a DC arc discharge device; placing a tungsten rod cathode and a copper pot anode relatively vertically; filling the reaction chamber with air, and passing circulating cooling water into the copper pot; operating a discharge reaction; collecting grayish yellow fluffy powder on a condensation wall as Eu 3+ Doped ZnO hierarchical nanostructure.

3. Eu according to claim 2 3+ The method for preparing a doped ZnO hierarchical nanostructure is characterized in that: In the method, the mixing molar ratio of Zn powder and Eu2O3 powder is 100:1-2.

4. Eu according to claim 2 3+ The method for preparing a doped ZnO hierarchical nanostructure is characterized in that: The air pressure in the reactor is 20-40 kPa.

5. Eu according to claim 2 3+ The method for preparing a doped ZnO hierarchical nanostructure is characterized in that: In the method, the reaction voltage is 20 to 30 V, the current is 60 to 80 A, and the reaction time is 10 to 30 seconds.

Citation Information

Patent Citations

  • Preparation of transient metal doped nano zinc oxide crystal whisker

    CN101498034A

  • Method for preparing metal zinc nanometer wire

    CN102139374A

  • Preparation method and application of europium-doped zinc oxide photocatalyst

    CN110280234A

  • Zinc Oxide Nanostructures and Sensors Using Zinc Oxide Nanostructures

    US20120091451A1