Polymer composite aggregate agent for ecological restoration of mining area and preparation method of polymer composite aggregate agent

By using polymer composite granules in mines, including modified lignin nanofibers and nanopore-sized breathable materials, the problem of insufficient stability and breathability of the granules on the steep slopes of the mine is solved, and the long-term stability and breathability of the soil are improved. , promotes vegetation growth.

CN118879332APending Publication Date: 2024-11-01ANHUI JINRISHENG MINING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410809195.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The granules on steep slopes in the mine are difficult to stabilize for a long time and have poor breathability, which leads to difficulty in breathing at the roots of plants and brings difficulties to the mine rejuvenation.

Method used

Using polymer composite granules, containing modified lignin nanofibers, nanopore-sized breathable materials, dispersants, polymer film forming agents, soil stabilizers and organic fertilizers, and cross-linking of modified lignin fibers The network improves the soil's water retention, fertilizer retention, breathability and stability, and prevents soil erosion.

Benefits of technology

Significantly improve the soil's water and fertilizer retention ability, stabilize the steep soil slopes for a long time, maintain the soil soft and breathable, prevent soil erosion, and improve the conditions for vegetation growth and reproduction.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a polymer composite aggregate agent for ecological restoration of a mining area and a preparation method of the polymer composite aggregate agent. The polymer composite aggregate agent is prepared from the following materials in percentage by weight: a polymer water-retaining agent, modified lignin nanofibers, a nano-aperture breathable material, a dispersing agent, a polymer film-forming agent, a soil stabilizer and an organic fertilizer. The lignin fibers are modified, the lignin fibers are refined under the assistance of acetic acid and a high-speed dispersion machine, and the long-term stability of the matrix on the abrupt slope can be greatly improved through a cross-linked network among the nanofibers; the nano-aperture breathable material can effectively improve the air permeability of the soil after spray-seeding so as to facilitate the growth and reproduction of vegetation, and meanwhile, due to the small aperture, the granular form of the soil after spray-seeding cannot be influenced; by adding the dispersing agent, the nano dispersion state of the modified lignin nanofiber and the nano-aperture breathable material is ensured. The alkyd resin disclosed by the invention can be subjected to self-crosslinking reaction in the air, so that the stability and rain wash resistance of the soil aggregate are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of environmental protection, and in particular to a polymer composite granule for ecological restoration of mining areas and a preparation method thereof. Background Art

[0002] The mining industry is one of the pillar industries of my country's national economy, providing a large amount of tax revenue and jobs for my country. However, the mining industry will bring a series of ecological and environmental problems such as soil erosion and serious secondary disasters. At present, the soil loss problem is mainly improved by using granulating agents. For example, CN103194241 B discloses a polymer granulating agent for high-order granulation spraying greening and its preparation method, which enables the soil to maintain an excellent granular structure. CN105993259B discloses a matrix material for ecological restoration of waste rock heaps in mining areas, and the granulating agent in the matrix material provides a good environment for plant growth.

[0003] However, there are a lot of steep slopes in mines, and it is difficult for the granular matrix to maintain long-term stability on the steep slopes after the granular agent is sprayed. At the same time, the air permeability of conventional granular agents is poor, which makes it difficult for the roots of plants to breathe, bringing great difficulties to the greening of mines.

[0004] Therefore, developing a mine ecological restoration granule that has both long-term stability on steep slopes and good air permeability is an urgent problem that needs to be solved by technicians in this field. Summary of the invention

[0005] The invention discloses a polymer composite granulating agent for ecological restoration of mining areas and a preparation method thereof, which can significantly improve the water-retaining, fertilizer-retaining and air-permeable capacity of soil, stabilize the granulation capacity of steep slopes of soil for a long term, maintain the softness and air-permeability of soil and prevent soil and water loss.

[0006] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a polymer composite granule for ecological restoration of mining areas, which is made of materials with the following weight ratios: 25-50 parts of polymer water retaining agent, 3-10 parts of modified lignin nanofibers, 2-5 parts of nanopore breathable materials, 1-2 parts of dispersant, 3-10 parts of polymer film-forming agent, 3-10 parts of soil stabilizer, and 3-10 parts of organic fertilizer.

[0007] Preferably, the method for preparing the modified lignin nanofiber comprises the following steps:

[0008] a. Dissolve acetic acid in water to prepare a 10wt% acetic acid solution;

[0009] b. Dissolve potassium hydroxide in ethanol to prepare a 0.1wt% potassium hydroxide ethanol solution;

[0010] c. Take an equal amount of lignin fiber as in step a and add it to the acetic acid solution, and disperse it in a high-speed disperser at a linear speed of 1-3 m / s; this operation is carried out in a water bath, the temperature of the water bath is controlled at 50-60°C, the reaction time is 2-5h, and it is naturally cooled to room temperature to obtain a solution;

[0011] d. The solution in step c is filtered, and then rinsed with the potassium hydroxide ethanol solution in step b until the pH value of the filtrate is 6.5;

[0012] e. Drying the solid in step d at room temperature to obtain modified lignin nanofibers.

[0013] Preferably, the method for preparing the nanopore breathable material comprises the following steps:

[0014] i. Dissolve 1,3,5-triformyl phloroglucinol in n-hexane to prepare a 20wt% 1,3,5-triformyl phloroglucinol n-hexane solution;

[0015] ii. dissolving m-phenylenediamine in water to prepare a 20wt% aqueous solution of m-phenylenediamine;

[0016] iii. The solution in step i and step ii are mixed in equal proportions, stirred in a stirrer at a stirring speed of 100-500 rpm / min; this operation is carried out in a water bath, the temperature of the water bath is controlled at 40-50°C, the reaction time is 48h, and naturally cooled to room temperature;

[0017] iv. The solution in step iii was filtered, dried, added to a 10 wt% acetic acid solution, and stirred at 50°C for 12 h;

[0018] v. The solution in step iv was filtered and rinsed with 0.1wt% potassium hydroxide ethanol solution until the pH value of the filtrate was 6.5;

[0019] v i. Drying the solid in step v at room temperature to obtain a nanopore breathable material.

[0020] Preferably, the polymer water-retaining agent is cationic polyacrylamide with a molecular weight of 8 million to 13 million.

[0021] Preferably, the dispersant is a silane coupling agent or a titanate coupling agent.

[0022] Preferably, the polymer film former is an alkyd resin with an oil length of >60%.

[0023] Preferably, the soil stabilizer is sodium carboxymethyl cellulose.

[0024] A method for preparing a polymer composite granule for ecological restoration of mining areas comprises the following steps:

[0025] (i) uniformly mixing 3-10 parts of modified lignin nanofibers, 2-5 parts of nanopore breathable materials, 1-2 parts of dispersants, and 3-10 parts of polymer film-forming agents to obtain a mixture; spraying anhydrous ethanol on the surface of the mixture until the surface of the mixture is wetted;

[0026] (ii) dissolving 25-50 parts of a polymer water retaining agent in water, and adding the wetted mixture in step (i) into the water, stirring evenly, to obtain a preparation for the granulating agent;

[0027] (iii) Add the prepared agent in step (ii) into the mixer of the spraying machine, add 3-10 parts of soil stabilizer and 3-10 parts of organic fertilizer at the same time, stir evenly, and then spraying can be carried out.

[0028] Preferably, the total solid content of the polymer composite granules during spraying is 0.1-1 wt%.

[0029] The beneficial effects of adopting the above technical solution are:

[0030] At present, conventional agglomerates are difficult to combine tightly with the soil, which makes the soil matrix after spraying easy to slide and difficult to maintain stably on the steep slope for a long time. The present invention modifies the lignin fibers. With the assistance of acetic acid and a high-speed disperser, the lignin fibers are refined. The refined modified lignin nanofibers have a strong affinity with the soil, and the cross-linked network between the nanofibers can greatly improve the long-term stability of the matrix on the steep slope.

[0031] The nano-pore air-permeable material of the present invention can effectively improve the air permeability of the soil after spraying, so as to facilitate the growth and reproduction of vegetation. At the same time, due to its tiny pore size, it will not affect the morphology of soil aggregates after spraying.

[0032] The addition of the dispersant in the present invention effectively ensures the nano-dispersion state of the modified lignin nano-fibers and the nano-pore size breathable material.

[0033] The alkyd resin in the present invention undergoes a self-crosslinking reaction in the air, thereby further improving the stability of soil aggregates and the ability to resist rainwater erosion. DETAILED DESCRIPTION

[0034] Embodiments of the present invention are described in detail below:

[0035] Example 1

[0036] A polymer composite granule for ecological restoration of mining areas, the preparation method of which comprises the following steps:

[0037] (i) 3 parts of modified lignin nanofibers, 2 parts of nanopore breathable materials, 1 part of a dispersant, wherein the dispersant is a silane coupling agent, and 3 parts of a polymer film-forming agent are mixed uniformly to obtain a mixture, wherein the polymer film-forming agent is an alkyd resin, and the oil length is 65%; anhydrous ethanol is sprayed on the surface of the mixture until the surface of the mixture is wetted;

[0038] (ii) dissolving 25 parts of a polymer water retaining agent in water, wherein the polymer water retaining agent is a cationic polyacrylamide with a molecular weight of 8 million, and then adding the wetted mixture in step (i) into the water, stirring evenly, to obtain a preparation for the granulating agent;

[0039] (iii) adding the preparation agent in step (ii) into the mixer of the spraying machine, adding 3 parts of soil stabilizer, wherein the soil stabilizer is sodium carboxymethyl cellulose, and 3 parts of organic fertilizer, stirring evenly, and then spraying can be carried out. The total solid content of the polymer composite granules for spraying is 0.1wt%.

[0040] The steps of preparing the modified lignin nanofibers include:

[0041] a. Dissolve acetic acid in water to prepare a 10wt% acetic acid solution;

[0042] b. Dissolve potassium hydroxide in ethanol to prepare a 0.1wt% potassium hydroxide ethanol solution;

[0043] c. Take an equal amount of lignin fiber as that in step a and add it to the acetic acid solution in step a, and disperse it in a high-speed disperser at a linear speed of 1 m / s; this operation is carried out in a water bath, the temperature of the water bath is controlled at 50°C, the reaction time is 2h, and it is naturally cooled to room temperature;

[0044] d. The solution in step c is filtered, and then rinsed with the potassium hydroxide ethanol solution in step b until the pH value of the filtrate is 6.5;

[0045] e. Drying the solid in step d at room temperature to obtain modified lignin nanofibers.

[0046] The preparation steps of the nanopore size breathable material include:

[0047] i. Dissolve 1,3,5-triformyl phloroglucinol in n-hexane to prepare a 20wt% 1,3,5-triformyl phloroglucinol n-hexane solution;

[0048] ii. dissolving m-phenylenediamine in water to prepare a 20wt% aqueous solution of m-phenylenediamine;

[0049] iii. The solution in step i and step ii was mixed in equal proportions, stirred in a stirrer at a stirring speed of 100 rpm / min; this operation was carried out in a water bath, the temperature of the water bath was controlled at 40°C, the reaction time was 48h, and naturally cooled to room temperature;

[0050] iv. The solution in step iii was filtered, dried, added to a 10 wt% acetic acid solution, and stirred at 50°C for 12 h;

[0051] v. The solution in step iv was filtered and rinsed with 0.1wt% potassium hydroxide ethanol solution until the pH value of the filtrate was 6.5;

[0052] v i. drying the solid in step v at room temperature to obtain a nanopore breathable material;

[0053] Example 2

[0054] A polymer composite granule for ecological restoration of mining areas, the preparation method of which comprises the following steps:

[0055] (i) 10 parts of modified lignin nanofibers, 5 parts of nanopore breathable materials, 2 parts of dispersants, wherein the dispersant is a titanate coupling agent, and 10 parts of polymer film-forming agents are mixed uniformly to obtain a mixture, wherein the polymer film-forming agent is an alkyd resin with an oil content of 70%; anhydrous ethanol is sprayed on the surface of the mixture until the surface of the mixture is wetted;

[0056] (ii) dissolving 50 parts of a polymer water retaining agent in water, wherein the polymer water retaining agent is a cationic polyacrylamide with a molecular weight of 13 million, and adding the wetted mixture in step (i) into the water, stirring evenly, to obtain a preparation for the granulating agent;

[0057] (iii) adding the preparation agent in step (ii) into the mixer of the spraying machine, adding 10 parts of soil stabilizer, wherein the soil stabilizer is sodium carboxymethyl cellulose, and 10 parts of organic fertilizer, stirring evenly, and then spraying can be carried out. The total solid content of the polymer composite granules for spraying is 1wt%.

[0058] The preparation steps of the modified lignin nanofibers include:

[0059] a. Dissolve acetic acid in water to prepare a 10wt% acetic acid solution;

[0060] b. Dissolve potassium hydroxide in ethanol to prepare a 0.1wt% potassium hydroxide ethanol solution;

[0061] c. Take an equal amount of lignin fiber as in step a and add it to the acetic acid solution in step a, and disperse it in a high-speed disperser at a linear speed of 3 m / s; this operation is carried out in a water bath, the temperature of the water bath is controlled at 60°C, the reaction time is 5h, and it is naturally cooled to room temperature;

[0062] d. The solution in step c is filtered, and then rinsed with the potassium hydroxide ethanol solution in step b until the pH value of the filtrate is 6.5;

[0063] e. Drying the solid in step d at room temperature to obtain modified lignin nanofibers.

[0064] The steps for preparing the nanopore breathable material include:

[0065] i. Dissolve 1,3,5-triformyl phloroglucinol in n-hexane to prepare a 20wt% 1,3,5-triformyl phloroglucinol n-hexane solution;

[0066] ii. dissolving m-phenylenediamine in water to prepare a 20wt% aqueous solution of m-phenylenediamine;

[0067] iii. Mix the solution in step i and step ii in equal proportions, stir in a stirrer at a stirring speed of 500 rpm / min. This operation is carried out in a water bath, the temperature of the water bath is controlled at 50°C, the reaction time is 48 hours, and naturally cool to room temperature;

[0068] iv. The solution in step iii was filtered, dried, added to a 10 wt% acetic acid solution, and stirred at 50°C for 12 h;

[0069] v. The solution in step iv was filtered and rinsed with 0.1wt% potassium hydroxide ethanol solution until the pH value of the filtrate was 6.5;

[0070] v i. Drying the solid in step v at room temperature to obtain a nanopore breathable material.

[0071] Example 3

[0072] A polymer composite granule for ecological restoration of mining areas, the preparation method of which comprises the following steps:

[0073] (i) 8 parts of modified lignin nanofibers, 3 parts of nanopore breathable materials, 2 parts of dispersants, wherein the dispersants are silane coupling agents, and 8 parts of polymer film-forming agents are mixed uniformly to obtain a mixture, wherein the polymer film-forming agent is an alkyd resin, and the oil length is 63%; anhydrous ethanol is sprayed on the surface of the mixture until the surface of the mixture is wetted;

[0074] (ii) dissolving 30 parts of a polymer water retaining agent in water, wherein the polymer water retaining agent is a cationic polyacrylamide with a molecular weight of 13 million, and adding the wetted mixture in step (i) into the water, stirring evenly, to obtain a preparation for the granulating agent;

[0075] (iii) adding the preparation agent in step (ii) into the mixer of the spraying machine, adding 8 parts of soil stabilizer, wherein the soil stabilizer is sodium carboxymethyl cellulose, and 8 parts of organic fertilizer, stirring evenly, and then spraying can be carried out. The total solid content of the polymer composite granules for spraying is 0.8wt%.

[0076] Wherein, the preparation steps of the modified lignin nanofiber are:

[0077] a. Dissolve acetic acid in water to prepare a 10wt% acetic acid solution;

[0078] b. Dissolve potassium hydroxide in ethanol to prepare a 0.1wt% potassium hydroxide ethanol solution;

[0079] c. Take an equal amount of lignin fiber to the acetic acid in step a and add it to the acetic acid solution in step a, and disperse it in a high-speed disperser at a linear speed of 2 m / s; this operation is carried out in a water bath, the temperature of the water bath is controlled at 55°C, the reaction time is 4h, and it is naturally cooled to room temperature;

[0080] d. The solution in step c is filtered, and then rinsed with the potassium hydroxide ethanol solution in step b until the pH value of the filtrate is 6.5;

[0081] e. Drying the solid in step d at room temperature to obtain modified lignin nanofibers.

[0082] The steps for preparing the nanopore breathable material include:

[0083] i. Dissolve 1,3,5-triformyl phloroglucinol in n-hexane to prepare a 20wt% 1,3,5-triformyl phloroglucinol n-hexane solution;

[0084] ii. dissolving m-phenylenediamine in water to prepare a 20wt% aqueous solution of m-phenylenediamine;

[0085] iii. Mix the solution in step i and step ii in equal proportions, stir in a stirrer at a stirring speed of 300 rpm / min. This operation is carried out in a water bath, the temperature of the water bath is controlled at 45°C, the reaction time is 48 hours, and naturally cool to room temperature;

[0086] iv. The solution in step iii was filtered, dried, added to a 10 wt% acetic acid solution, and stirred at 50°C for 12 h;

[0087] v. The solution in step iv was filtered and rinsed with 0.1wt% potassium hydroxide ethanol solution until the pH value of the filtrate was 6.5;

[0088] v i. Drying the solid in step v at room temperature to obtain a nanopore breathable material.

[0089] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several modifications and improvements without departing from the inventive concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A polymer composite granule for ecological restoration of mining areas, characterized in that: The invention is made of materials in the following weight proportions: 25-50 parts of polymer water retaining agent, 3-10 parts of modified lignin nanofiber, 2-5 parts of nanopore breathable material, 1-2 parts of dispersant, 3-10 parts of polymer film-forming agent, 3-10 parts of soil stabilizer and 3-10 parts of organic fertilizer.

2. The polymer composite granule for ecological restoration of mining areas according to claim 1, characterized in that: The preparation method of the modified lignin nanofiber comprises the following steps: a. Dissolve acetic acid in water to prepare a 10wt% acetic acid solution; b. Dissolve potassium hydroxide in ethanol to prepare a 0.1wt% potassium hydroxide ethanol solution; c. Take an equal amount of lignin fiber as in step a and add it to the acetic acid solution, and disperse it in a high-speed disperser at a linear speed of 1-3 m / s; this operation is carried out in a water bath, the temperature of the water bath is controlled at 50-60°C, the reaction time is 2-5h, and it is naturally cooled to room temperature to obtain a solution; d. The solution in step c is filtered, and then rinsed with the potassium hydroxide ethanol solution in step b until the pH value of the filtrate is 6.5; e. Drying the solid in step d at room temperature to obtain modified lignin nanofibers.

3. The polymer composite granule for ecological restoration of mining areas according to claim 1, characterized in that: The preparation method of the nanopore size breathable material comprises the following steps: i. Dissolve 1,3,5-triformyl phloroglucinol in n-hexane to prepare a 20wt% 1,3,5-triformyl phloroglucinol n-hexane solution; ii. dissolving m-phenylenediamine in water to prepare a 20wt% aqueous solution of m-phenylenediamine; iii. The solution in step i and step ii are mixed in equal proportions, stirred in a stirrer at a stirring speed of 100-500 rpm / min; this operation is carried out in a water bath, the temperature of the water bath is controlled at 40-50°C, the reaction time is 48h, and naturally cooled to room temperature; iv. The solution in step iii was filtered, dried and added to a 10 wt % acetic acid solution and stirred at 50 ° C for 12 h; v. The solution in step iv was filtered and rinsed with 0.1wt% potassium hydroxide ethanol solution until the pH value of the filtrate was 6.5; vi. Dry the solid in step v at room temperature to obtain a nanopore breathable material.

4. The polymer composite granule for ecological restoration of mining areas according to claim 1, characterized in that: The polymer water-retaining agent is a cationic polyacrylamide with a molecular weight of 8 million to 13 million.

5. The polymer composite granule for ecological restoration of mining areas according to claim 1, characterized in that: The dispersant is a silane coupling agent or a titanate coupling agent.

6. The polymer composite granule for ecological restoration of mining areas according to claim 1, characterized in that: The polymer film former is alkyd resin with oil content > 60%.

7. The polymer composite granule for ecological restoration of mining areas according to claim 1, characterized in that: The soil stabilizer is sodium carboxymethyl cellulose.

8. A method for preparing a polymer composite granule for ecological restoration of mining areas according to any one of claims 1 to 7, comprising the following steps: (i) uniformly mixing 3-10 parts of modified lignin nanofibers, 2-5 parts of nanopore breathable materials, 1-2 parts of dispersants, and 3-10 parts of polymer film-forming agents to obtain a mixture; spraying anhydrous ethanol on the surface of the mixture until the surface of the mixture is wetted; (ii) dissolving 25-50 parts of a polymer water retaining agent in water, and adding the wetted mixture in step (i) into the water, stirring evenly, to obtain a preparation for a granulating agent; (iii) Add the prepared agent in step (ii) into the mixer of the spraying machine, add 3-10 parts of soil stabilizer and 3-10 parts of organic fertilizer at the same time, stir evenly, and then spraying can be carried out.

9. The polymer composite granule for ecological restoration of mining areas according to claim 8, characterized in that: The total solid content of the polymer composite granules during spraying is 0.1-1wt%.