Process technology for improving leather yield
Through multiple de-ashing and softening operations, the problem of gray skin swelling in leather processing hindering re-ashing is solved, which significantly improves the leather yield and softness of the leather, and is suitable for a variety of leather processes.
Patent Information
- Application Number
- CN202410957243.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-01
AI Technical Summary
During the leather processing, the alkali-expanded gray peel prevents the compound ash material from penetrating into the skin core and microfibers again due to the ionic effect, resulting in poor re-ashing effect and affecting the leather yield rate.
Through multiple de-ashing and softening operations, the gray skin swells are eliminated and the ash alkali material is fully penetrated, making the fiber dispersion effect more obvious and increasing the leather margin rate. The specific steps include first deaze, first softening, re-ashing, deaze, and softening, and cycle to improve the ash alkali treatment effect.
Significantly increase the leather margin rate, reduce gray leather patterns, improve the softness and feel of the leather, and is suitable for sofas, clothing and soft upper blue leather crafts.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of leather processing, in particular to a process technology for improving the leather yield. Background Art
[0002] Leather is an important natural fabric for making clothing, shoe uppers and bags, etc. Its good durability and natural texture are highly accepted by consumers. In the leather processing process, the soft and comfortable style is mainly obtained by separating and dispersing the natural leather fibers with ash alkali. At the same time, the effect of this process has a great influence on the leather yield. The relevant process usually obtains a certain degree of fiber dispersion and separation effect through the liming-reliming process. However, the effect of reliming the leather fibers after ash alkali expansion is poor. This is mainly because the ash leather after alkali expansion prevents the reliming material from penetrating into the leather core and microfibers again due to the ion effect, which inhibits the reliming effect. Therefore, how to further improve the leather yield by improving the ash alkali treatment steps is a problem that the existing technical staff urgently needs to solve. Summary of the invention
[0003] The purpose of the present invention is to provide a process technology for improving the leather yield, so as to solve the above-mentioned problems in the background technology. The leather ash alkali treatment method designed by the present invention can effectively increase the effect of the re-ashing effect, significantly reduce the gray leather grain, increase the softness of the leather, make the leather grain more open, feel better, and significantly increase the leather yield. This process is suitable for the production of blue leather processes for sofas, clothing and soft shoe uppers.
[0004] To achieve the above object, the present invention provides the following technical solutions:
[0005] One of the technical solutions of the present invention is to provide a leather ash alkali treatment method for improving the leather yield of leather, which comprises the following steps in sequence:
[0006] The lime skin obtained after liming is taken and subjected to the first deliming, the first softening, the reliming, the deliming and the softening to complete the ash alkali treatment steps.
[0007] Preferably, the first deliming step is: at 26-28° C., the lime skin obtained after liming and water are mixed in a drum in a mass ratio of 1:1-2, and then 0.4-0.5wt% of deliming agent SINOBEAM DL22 and 0.5-0.6wt% of ammonium sulfate are added, and the mixture is rotated for 20 minutes, and then 0.5-0.6wt% of ammonium sulfate is added, and the mixture is rotated for 40 minutes;
[0008] The deliming step comprises: mixing the leather obtained after reliming and water in a drum at a mass ratio of 1:1-2 at 26-28° C., then adding 0.4-0.5wt% of deliming agent SINOBEAM DL22 and 0.5-0.6wt% of ammonium sulfate, rotating for 20 minutes, and then adding 0.5-0.6wt% of ammonium sulfate, rotating for 40 minutes.
[0009] Preferably, the first softening step is: adding 0.3-0.5wt% of softening enzyme NS to the reaction system after the first deliming, rotating for 20 minutes, controlling the liquid at pH=6.5-7.5, and washing twice with normal temperature water;
[0010] The softening step is: adding 0.3-0.5wt% softening enzyme NS to the delimed reaction system, rotating for 20 minutes, controlling the liquid at pH=6.5-7.5, and washing twice with normal temperature water.
[0011] Preferably, the step of reliming is: mixing the softened leather with the reliming liquid and soaking; the soaking temperature is 18-22°C, the time is 24-48h, the mass ratio of the reliming liquid to the leather is 200-300%, and the drum rotation frequency during soaking is 3-5min per hour.
[0012] Preferably, the liming solution comprises, by mass percentage, 0.2-1.0% of liming agent SINOBEAM LM, 2-8% of lime, 0-0.5% of alkali sulfide and not 0, and the balance is water.
[0013] Preferably, after the lime restoration, deliming and softening operations are completed, the method further comprises the step of cyclically performing the lime restoration, deliming and softening operations at least once.
[0014] The second technical solution of the present invention is to provide a leather material treated with ash and alkali obtained according to the above leather ash and alkali treatment method.
[0015] The third technical solution of the present invention is to provide an application of the above leather ash alkali treatment method in improving the leather yield.
[0016] The beneficial technical effects of the present invention are as follows:
[0017] The present invention eliminates the expansion of the ash skin by deliming and softening, and then performs a reliming operation, so that the expanded material can fully penetrate into the leather collagen fiber bundles, and the leather fibers are subjected to multiple effective liming and alkali actions, so that the fiber dispersion and separation effects are more obvious, and the leather yield is significantly increased. This is mainly due to the multiple deliming and softening operations, which significantly eliminate the expansion of the ash skin and help the liming and alkali materials to fully penetrate again. At the same time, the collagen three-dimensional spiral structure of the fiber is destroyed to a certain extent in the early liming and deliming treatment process, which is more conducive to the full separation and loosening effect of the secondary liming and alkali, and the liming and alkali treatment effect is improved.
[0018] This process can effectively increase the effect of ash alkali, fully loosen and separate fibers, reduce gray leather grain, increase leather softness, make leather grain more open, feel better, and significantly increase leather yield. This process is suitable for the production of blue leather for sofas, clothing and soft shoe uppers.
[0019] The leather ash alkali treatment method designed by the invention can obtain an area increase rate of at least 10% under the condition of using the same ash alkali amount and action time, and at the same time give the leather a softer, more velvety and fuller feel. DETAILED DESCRIPTION
[0020] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.
[0021] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0022] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.
[0023] The words “include,” “including,” “have,” “contain,” etc. used in the present invention are open-ended terms, meaning including but not limited to.
[0024] All raw materials used in the following examples and comparative examples of the present invention are commercially available products.
[0025] Unless otherwise specified, "overnight" in the present invention is calculated as 12 hours.
[0026] The "normal temperature" in the present invention is 22°C unless otherwise specified.
[0027] Unless otherwise specified, the "liquid ratio" in the present invention is calculated based on the mass ratio of the liquid phase component in the drum to the leather material.
[0028] The raw material skins used in the following examples and comparative examples of the present invention were weighed after fully removing the salt, which was used as the basis for measurement.
[0029] The percentages of the various raw materials described in the following embodiments and comparative examples of the present invention are all calculated based on the mass percentage of the various raw materials to the leather material.
[0030] Example 1
[0031] Preparation of Yellow Bull Nappa Upper Leather:
[0032] (1) Pre-soaking: At 20-22°C, water and raw hides are put into a drum in a mass ratio of 300%, 0.1% fungicide XJ150 is added, the drum is rotated for 5 minutes, and then left to stand overnight, and then rotated for 5 minutes every hour thereafter, for a total of 6 hours, and then the solution in the drum is discharged.
[0033] (2) Water washing: Add water equivalent to 300% of the leather mass into the drum again, rotate for 10 minutes, and then drain the solution in the drum.
[0034] (3) Re-washing: Add 300% of the leather mass of water into the drum again, rotate for 10 minutes, and then drain the solution in the drum.
[0035] (4) Main immersion: The main immersion liquid is prepared according to the following mass percentages: 0.15% immersion agent SINOBEAM SA, 0.15% bactericide SINOBEAM XJ150, 0.2% degreasing agent SINOBEAM DG, and the balance is water.
[0036] Add the main soaking liquid equivalent to 300% of the leather mass into the drum, rotate for 20 minutes, let it stand for 40 minutes, and then rotate for 3 minutes every hour, for a total of 18 hours; among them, add 0.15% of the fungicide SINOBEAM XJ150 after 6 hours of circulation. After the cycle is completed, rotate for 10 minutes, and then drain the liquid and take out the leather.
[0037] (5) Meat removal: Use a meat remover to remove the meat.
[0038] (6) Degreasing: The degreasing liquid is prepared according to the following mass percentages: 0.5% of degreasing agent SINOBEAM DG, 0.3% of oil dispersant SINOIL MZ, and the balance is water.
[0039] At 40°C, mix the degreasing liquid and leather in a drum at a mass ratio of 300%, rotate for 20 minutes, stop for 20 minutes, rotate for 20 minutes, drain the liquid, add 40°C water to wash for 5 minutes, wash with running water for 5 minutes, and drain the liquid.
[0040] (7) Secondary immersion: The secondary immersion liquid is prepared according to the following mass percentages: 0.2% immersion agent SINOBEAM SA, 0.2% bactericide SINOBEAM XJ150, 0.2% degreasing agent SINOBEAM DG, and the balance is water.
[0041] At 20-22℃, add 300% of the secondary soaking liquid of the leather mass into the drum, rotate for 20 minutes, let it stand for 40 minutes, and then rotate for 3 minutes every hour, for a total of 18 hours; after 6 hours of circulation, add 0.15% of the fungicide SINOBEAM XJ150. After the cycle is completed, rotate for 10 minutes, and then drain the liquid and take out the leather.
[0042] (8) Hair removal and liming:
[0043] At 22°C, add 300% of the weight of the leather into the drum, wash it with water for 5 minutes, drain some of the water to make the weight ratio of water to leather 100%, add 0.8% sodium hydrosulfide and 1.2% liming agent SINOBEAMLM, then rotate for 40 minutes, stop for 30 minutes, then add 1.6% alkali sulfide, 0.2% sodium hydrosulfide, 1.5% lime powder, rotate for 10 minutes, stop for 20 minutes, repeat 5 times (total time 150 minutes), add 0.4% CR and 1.5% lime powder, rotate for 10 minutes, stop for 20 minutes, repeat 4 times (total time 120 minutes), add water to the liquid ratio of 250%, continue to rotate for 30 minutes, stop for 30 minutes, rotate for 10 minutes, stop the drum, then cycle 6 times in a way of rotating for 3 minutes per hour, and drain the liquid.
[0044] (9) First deliming, first softening and reliming: At 26-28°C, add water equivalent to 100% of the leather mass into a rotating drum, then add 0.4% of deliming agent SINOBEAM DL22 and 0.5% of ammonium sulfate, rotate for 20 minutes, then add 0.5% of ammonium sulfate, rotate for 40 minutes, then add 0.3% of softening enzyme NS, rotate for 20 minutes, control the liquid at pH = 6.5-7.5, rinse twice with normal temperature water, and drain.
[0045] The liming solution is prepared according to the following mass percentages: liming agent SINOBEAM LM 0.5%, lime 2%, sodium sulfide 0.5%, and the balance is water.
[0046] At room temperature, add 300% of the leather mass of the lime solution into the drum, rotate for 120 minutes, then circulate for 24 hours at a rotation rate of 3 minutes per hour, and drain the liquid.
[0047] (10) Secondary deliming and secondary softening: At 26-28°C, add water equivalent to 100% of the leather mass into a rotating drum, then add 0.4% of deliming agent SINOBEAM DL22 and 0.6% of ammonium sulfate, rotate for 20 minutes, then add 0.6% of ammonium sulfate, rotate for 40 minutes, then add 0.3% of softening enzyme NS, rotate for 20 minutes, control the liquid at pH = 6.5-7.5, rinse twice with room temperature water, and drain.
[0048] (11) Pickling: At room temperature, add water equivalent to 100% of the hide mass into a rotating drum, then add 6% salt, and then add sulfuric acid (dilute sulfuric acid and water at a ratio of 1:10, cool, and add three times at intervals of 20 minutes) to adjust the pH to 2.8-3.0, rotate for 90 minutes, and drain.
[0049] (12) Tanning: 6.5% chromium powder, rotate for 3 hours and check
[0050] MgO 0.3% Rotation 60 minutes
[0051] Water 200%, internal temperature 38 ℃, rotate for 5 hours, take out of the drum and let it stand to obtain blue skin.
[0052] Comparative Example 1
[0053] The only difference from Example 1 is that step (9) and step (10) are omitted and modified as follows:
[0054] (9) Reliming: Prepare the reliming solution according to the following mass percentages: liming agent SINOBEAM LM 0.5%, lime 2%, sodium sulfide 0.5%, and the balance water.
[0055] At room temperature, add 300% of the weight of the leather into the drum, rotate for 120 minutes, then circulate for 24 hours at a rotation rate of 5 minutes per hour, and drain the liquid.
[0056] (10) Deliming and softening: At 26-28°C, add water equivalent to 100% of the leather mass into a rotating drum, then add 0.4% of deliming agent SINOBEAM DL22 and 0.5% of ammonium sulfate, rotate for 20 minutes, then add 0.5% of ammonium sulfate, rotate for 40 minutes, then add 0.6% of softening enzyme NS, rotate for 40 minutes, control the liquid at pH = 6.5-7.5, rinse twice with normal temperature water, and drain.
[0057] The test showed that compared with comparative example 1, the blue leather area of example 1 increased by 16.75%, and the leather tensile strength was 37.6 N / mm 2 , compared with 38.9N / mm in Comparative Example 1 2 near.
[0058] Example 2
[0059] Preparation of yellow cattle sofa leather:
[0060] (1) Pre-soaking: At 20-22°C, water and raw hides are put into a drum in a mass ratio of 300%, 0.1% fungicide XJ150 is added, the drum is rotated for 5 minutes, and then left to stand overnight, and then rotated for 5 minutes every hour thereafter, for a total of 6 hours, and then the solution in the drum is discharged.
[0061] (2) Water washing: Add water equivalent to 300% of the leather mass into the drum again, rotate for 10 minutes, and then drain the solution in the drum.
[0062] (3) Re-washing: Add 300% of the leather mass of water into the drum again, rotate for 10 minutes, and then drain the solution in the drum.
[0063] (4) Main immersion: The main immersion liquid is prepared according to the following mass percentages: 0.15% immersion agent SINOBEAM SA, 0.15% bactericide SINOBEAM XJ150, 0.2% degreasing agent SINOBEAM DG, and the balance is water.
[0064] Add the main soaking liquid equivalent to 300% of the leather mass into the drum, rotate for 20 minutes, let it stand for 40 minutes, and then rotate for 3 minutes every hour, for a total of 18 hours; among them, add 0.15% of the fungicide SINOBEAM XJ150 after 6 hours of circulation. After the cycle is completed, rotate for 10 minutes, and then drain the liquid and take out the leather.
[0065] (5) Remove the meat: Use a meat remover.
[0066] (6) Degreasing: The degreasing liquid is prepared according to the following mass percentages: 0.5% of degreasing agent SINOBEAM DG, 0.3% of oil dispersant SINOIL MZ, and the balance is water.
[0067] At 40°C, mix the degreasing liquid and leather in a rotating drum at a mass ratio of 300% to the raw leather, rotate for 20 minutes, stop for 20 minutes, rotate for 20 minutes, drain the liquid, add 40°C water to wash for 5 minutes, wash with running water for 5 minutes, and drain the liquid.
[0068] (7) Secondary immersion: The secondary immersion liquid is prepared according to the following mass percentages: 0.2% immersion agent SINOBEAM SA, 0.2% bactericide SINOBEAM XJ150, 0.2% degreasing agent SINOBEAM DG, and the balance is water.
[0069] At 20-22℃, add 300% of the secondary soaking liquid of the leather mass into the drum, rotate for 20 minutes, let it stand for 40 minutes, and then rotate for 3 minutes every hour, for a total of 18 hours; after 6 hours of circulation, add 0.15% of the fungicide SINOBEAM XJ150. After the cycle is completed, rotate for 10 minutes, and then drain the liquid and take out the leather.
[0070] (8) Hair removal and liming:
[0071] At 22°C, add 300% of the weight of the leather into the drum, wash it with water for 5 minutes, drain some of the water to make the weight ratio of water to leather 100%, add 0.8% sodium hydrosulfide and 1.2% liming agent SINOBEAMLM, then rotate for 40 minutes, stop for 30 minutes, then add 1.6% alkali sulfide, 0.2% sodium hydrosulfide, 1.5% lime powder, rotate for 10 minutes, stop for 20 minutes, repeat 5 times (total time 150 minutes), add 0.4% CR and 1.5% lime powder, rotate for 10 minutes, stop for 20 minutes, repeat 4 times (total time 120 minutes), add water to the liquid ratio of 250%, continue to rotate for 30 minutes, stop for 30 minutes, rotate for 10 minutes, stop the drum, then cycle 6 times in a way of rotating for 3 minutes per hour, and drain the liquid.
[0072] (9) Initial deliming, softening and reliming: At 26-28°C, add water equivalent to 100% of the leather mass into a rotating drum, then add 0.4% of deliming agent SINOBEAM DL22 and 0.5% of ammonium sulfate, rotate for 20 minutes, then add 0.5% of ammonium sulfate, rotate for 40 minutes, then add 0.3% of softening enzyme NS, rotate for 20 minutes, control the liquid at pH = 6.5-7.5, rinse twice with normal temperature water, and drain.
[0073] The liming solution is prepared according to the following mass percentages: liming agent SINOBEAM LM 0.5%, lime 3%, sodium sulfide 0.5%, and the balance is water.
[0074] At room temperature, add 300% of the leather mass of the lime solution into the drum, rotate for 120 minutes, then circulate for 24 hours at a rotation rate of 3 minutes per hour, and drain the liquid.
[0075] (10) Secondary deliming and softening: At 26-28°C, add water equivalent to 100% of the leather mass into a rotating drum, then add 0.4% of deliming agent SINOBEAM DL22 and 0.6% of ammonium sulfate, rotate for 20 minutes, then add 0.6% of ammonium sulfate, rotate for 40 minutes, then add 0.3% of softening enzyme NS, rotate for 20 minutes, control the liquid at pH = 6.5-7.5, rinse twice with normal temperature water, and drain.
[0076] Secondary reliming: Prepare the reliming liquid according to the following mass percentages: liming agent SINOBEAM LM 0.5%, lime 4%, sodium sulfide 0.5%, and the balance water.
[0077] At room temperature, add 300% of the leather mass of the lime solution into the drum, rotate for 120 minutes, then circulate for 24 hours at a rotation rate of 3 minutes per hour, and drain the liquid.
[0078] Three-time deliming and softening: at 26-28℃, add water equivalent to 100% of the leather mass into the drum, then add deliming agent SINOBEAM DL220.4%, ammonium sulfate 0.6%, rotate for 20 minutes, then add ammonium sulfate 0.6%, rotate for 40 minutes, then add softening enzyme NS 0.3%, rotate for 20 minutes, control the liquid at pH=6.5-7.5, wash twice with normal temperature water, and drain.
[0079] (11) Pickling: At room temperature, add water equivalent to 100% of the hide mass into a rotating drum, then add 6% salt, and then add sulfuric acid (dilute sulfuric acid and water at a ratio of 1:10, cool, and add three times at intervals of 20 minutes) to adjust the pH to 2.8-3.0, rotate for 90 minutes, and drain.
[0080] (12) Tanning: 6.5% chromium powder, rotate for 3 hours and check
[0081] MgO 0.3% Rotation 60 minutes
[0082] Water 200%, internal temperature 38 ℃, rotate for 5 hours, take out of the drum and let it stand to obtain blue skin.
[0083] Comparative Example 2
[0084] The only difference from Example 2 is that step (9) and step (10) are omitted and modified as follows:
[0085] (9) Reliming: Prepare the reliming liquid according to the following mass ratio: liming agent SINOBEAM LM 1.0%, lime 7%, sodium sulfide 1.0%, and the balance water.
[0086] At room temperature, add 300% of the leather mass into the drum, rotate for 120 minutes, then circulate for 48 hours at a rotation rate of 3 minutes per hour, and drain the liquid.
[0087] (10) Deliming and softening: At 26-28°C, add water equivalent to 100% of the leather mass into a rotating drum, then add 0.4% of deliming agent SINOBEAM DL22 and 0.5% of ammonium sulfate, rotate for 20 minutes, then add 0.5% of ammonium sulfate, rotate for 40 minutes, then add 0.9% of softening enzyme NS, rotate for 60 minutes, control the liquid at pH = 6.5-7.5, rinse twice with normal temperature water, and drain.
[0088] The test showed that compared with comparative example 2, the blue leather area of example 2 increased by 20.37%, and the leather tensile strength was 33.6 N / mm 2 , compared with 35.2N / mm in Comparative Example 2 2 near.
[0089] Example 3
[0090] Preparation of yak clothing leather:
[0091] (1) Pre-soaking: At 20-22°C, water and raw hides are put into a drum in a mass ratio of 300%, 0.1% fungicide XJ150 is added, the drum is rotated for 5 minutes, and then left to stand overnight, and then rotated for 5 minutes every hour thereafter, for a total of 6 hours, and then the solution in the drum is discharged.
[0092] (2) Water washing: Add water equivalent to 300% of the leather mass into the drum again, rotate for 10 minutes, and then drain the solution in the drum.
[0093] (3) Re-washing: Add 300% of the leather mass of water into the drum again, rotate for 10 minutes, and then drain the solution in the drum.
[0094] (4) Main immersion: The main immersion liquid is prepared according to the following mass ratio: 0.15% immersion agent SINOBEAM SA, 0.15% bactericide SINOBEAM XJ150, 0.2% degreasing agent SINOBEAM DG, and the balance is water.
[0095] Add the main soaking liquid equivalent to 300% of the leather mass into the drum, rotate for 20 minutes, let it stand for 40 minutes, and then rotate for 3 minutes every hour, for a total of 18 hours; among them, add 0.15% of the fungicide SINOBEAM XJ150 after 6 hours of circulation. After the cycle is completed, rotate for 10 minutes, and then drain the liquid and take out the leather.
[0096] (5) Remove the meat: Use a meat remover.
[0097] (6) Degreasing: The degreasing liquid is prepared according to the following mass percentages: 0.5% of degreasing agent SINOBEAM DG, 0.3% of oil dispersant SINOIL MZ, and the balance is water.
[0098] At 40°C, mix the degreasing liquid and leather in a drum at a mass ratio of 300%, rotate for 20 minutes, stop for 20 minutes, rotate for 20 minutes, drain the liquid, add 40°C water to wash for 5 minutes, wash with running water for 5 minutes, and drain the liquid.
[0099] (7) Secondary immersion: The secondary immersion liquid is prepared according to the following mass percentages: 0.2% immersion agent SINOBEAM SA, 0.2% bactericide SINOBEAM XJ150, 0.2% degreasing agent SINOBEAM DG, and the balance is water.
[0100] At 20-22℃, add 300% of the secondary soaking liquid of the leather mass into the drum, rotate for 20 minutes, let it stand for 40 minutes, and then rotate for 3 minutes every hour, for a total of 18 hours; after 6 hours of circulation, add 0.15% of the fungicide SINOBEAM XJ150. After the cycle is completed, rotate for 10 minutes, and then drain the liquid and take out the leather.
[0101] (8) Hair removal and liming:
[0102] At 22°C, add 300% of the weight of the leather into the drum, wash it with water for 5 minutes, drain some of the water to make the weight ratio of water to leather 100%, add 0.8% sodium hydrosulfide and 1.2% liming agent SINOBEAMLM, then rotate for 40 minutes, stop for 30 minutes, then add 1.6% alkali sulfide, 0.2% sodium hydrosulfide, 1.5% lime powder, rotate for 10 minutes, stop for 20 minutes, repeat 5 times (total time 150 minutes), add 0.4% CR and 1.5% lime powder, rotate for 10 minutes, stop for 20 minutes, repeat 4 times (total time 120 minutes), add water to the liquid ratio of 250%, continue to rotate for 30 minutes, stop for 30 minutes, rotate for 10 minutes, stop the drum, then cycle 6 times in a way of rotating for 3 minutes per hour, and drain the liquid.
[0103] (9) Initial deliming, softening and reliming: At 26-28°C, add water equivalent to 100% of the leather mass into a rotating drum, then add 0.4% of deliming agent SINOBEAM DL22 and 0.5% of ammonium sulfate, rotate for 20 minutes, then add 0.5% of ammonium sulfate, rotate for 40 minutes, then add 0.3% of softening enzyme NS, rotate for 20 minutes, control the liquid at pH = 6.5-7.5, rinse twice with normal temperature water, and drain.
[0104] The liming solution is prepared according to the following mass percentages: liming agent SINOBEAM LM 0.5%, lime 4%, sodium sulfide 0.5%, and the balance is water.
[0105] At room temperature, add 300% of the leather mass of the lime solution into the drum, rotate for 120 minutes, then circulate for 24 hours at a rotation rate of 3 minutes per hour, and drain the liquid.
[0106] (10) Secondary deliming and softening: At 26-28°C, add water equivalent to 100% of the leather mass into a rotating drum, then add 0.4% of deliming agent SINOBEAM DL22 and 0.6% of ammonium sulfate, rotate for 20 minutes, then add 0.6% of ammonium sulfate, rotate for 40 minutes, then add 0.3% of softening enzyme NS, rotate for 20 minutes, control the liquid at pH = 6.5-7.5, rinse twice with normal temperature water, and drain.
[0107] Secondary reliming: Prepare the reliming liquid according to the following mass ratio: liming agent SINOBEAM LM 0.5%, lime 2%, sodium sulfide 0.5%, and the balance is water.
[0108] At room temperature, add 300% of the weight of the leather into the drum, rotate for 120 minutes, then circulate for 24 hours at a rotation rate of 5 minutes per hour, and drain the liquid.
[0109] Three-time deliming and softening: at 26-28℃, add water equivalent to 100% of the leather mass into the drum, then add deliming agent SINOBEAM DL220.4%, ammonium sulfate 0.6%, rotate for 20 minutes, then add ammonium sulfate 0.6%, rotate for 40 minutes, then add softening enzyme NS 0.3%, rotate for 20 minutes, control the liquid at pH=6.5-7.5, wash twice with normal temperature water, and drain.
[0110] Third reliming: prepare the reliming liquid according to the following mass ratio: liming agent SINOBEAM LM 0.2%, lime 2%, sodium sulfide 0.2%, and the balance is water.
[0111] At room temperature, add 300% of the weight of the leather into the drum, rotate for 120 minutes, then circulate for 24 hours at a rotation rate of 5 minutes per hour, and drain the liquid.
[0112] Four times of deliming and softening: at 26-28℃, add water equivalent to 100% of the leather mass into the drum, then add deliming agent SINOBEAM DL220.4%, ammonium sulfate 0.6%, rotate for 20 minutes, then add ammonium sulfate 0.6%, rotate for 40 minutes, then add softening enzyme NS 0.3%, rotate for 20 minutes, control the liquid at pH=6.5-7.5, wash twice with normal temperature water, and drain.
[0113] (11) Pickling: At room temperature, add water equivalent to 100% of the hide mass into a rotating drum, then add 6% salt, and then add sulfuric acid (dilute sulfuric acid and water at a ratio of 1:10, cool, and add three times at intervals of 20 minutes) to adjust the pH to 2.8-3.0, rotate for 90 minutes, and drain.
[0114] (12) Tanning: 6.5% chromium powder, rotate for 3 hours and check
[0115] MgO 0.3% Rotation 60 minutes
[0116] Water 200%, internal temperature 38 ℃, rotate for 5 hours, take out of the drum and let it stand to obtain blue skin.
[0117] Comparative Example 3
[0118] The only difference from Example 3 is that step (9) and step (10) are omitted and modified as follows:
[0119] (9) Reliming: Prepare the reliming liquid according to the following mass ratio: liming agent SINOBEAM LM 1.2%, lime 8%, sodium sulfide 1.2%, and the balance water.
[0120] At room temperature, add 300% of the weight of the leather into the drum, rotate for 120 minutes, then circulate for 72 hours at a rotation rate of 3 minutes per hour, and drain the liquid.
[0121] (10) Deliming and softening: At 26-28°C, add water equivalent to 100% of the leather mass into a rotating drum, then add 0.4% of deliming agent SINOBEAM DL22 and 0.5% of ammonium sulfate, rotate for 20 minutes, then add 0.5% of ammonium sulfate, rotate for 40 minutes, then add 1.2% of softening enzyme NS, rotate for 80 minutes, control the liquid at pH = 6.5-7.5, rinse twice with normal temperature water, and drain.
[0122] The test showed that compared with comparative example 3, the blue leather area of example 3 increased by 26.50%, and the leather tensile strength was 27.3 N / mm 2 , compared with 30.2N / mm in Comparative Example 3 2 near.
[0123] It can be seen that the new ash alkali process will cause the leather strength to decrease slightly compared with the traditional process, but the degree is limited.
[0124] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for treating leather with ash alkali to improve the leather yield, characterized in that: The following steps are included in sequence: The lime skin obtained after liming is taken and subjected to the first deliming, the first softening, the reliming, the deliming and the softening to complete the ash alkali treatment steps.
2. The leather ash alkali treatment method according to claim 1, characterized in that: The step of reliming is: mixing the softened leather with the reliming liquid and soaking; the soaking temperature is 18-22°C, the time is 24-48h, the mass ratio of the reliming liquid to the leather is 200-300%, and the rotation frequency of the drum during soaking is 3-5min per hour.
3. The leather ash alkali treatment method according to claim 2, characterized in that, In terms of mass percentage, the liming liquid comprises: 0.2-1.0% of liming agent SINOBEAM LM, 2-8% of lime, 0-0.5% of sodium sulfide and not 0, and the balance is water.
4. The leather ash alkali treatment method according to claim 1, characterized in that: The first deliming step is: at 26-28° C., the lime skin obtained after liming and water are mixed in a drum in a mass ratio of 1:1-2, and then 0.4-0.5wt% of deliming agent SINOBEAM DL22 and 0.5-0.6wt% of ammonium sulfate are added, and the drum is rotated for 20 minutes, and then 0.5-0.6wt% of ammonium sulfate is added, and the drum is rotated for 40 minutes; The deliming step comprises: mixing the leather obtained after reliming and water in a drum at a mass ratio of 1:1-2 at 26-28° C., then adding 0.4-0.5wt% of deliming agent SINOBEAM DL22 and 0.5-0.6wt% of ammonium sulfate, rotating for 20 minutes, and then adding 0.5-0.6wt% of ammonium sulfate, rotating for 40 minutes.
5. The leather ash alkali treatment method according to claim 1, characterized in that: The first softening step is: adding softening enzyme NS 0.3-0.5wt% to the reaction system after the first deliming, rotating for 20 minutes, controlling the liquid at pH = 6.5-7.5, and washing with normal temperature water twice; The softening step is: adding 0.3-0.5wt% softening enzyme NS to the delimed reaction system, rotating for 20 minutes, controlling the liquid at pH=6.5-7.5, and washing twice with normal temperature water.
6. The leather ash alkali treatment method according to claim 1, characterized in that: After the lime-replenishing, deliming and softening operations are completed, the method further comprises the step of cyclically performing the lime-replenishing, deliming and softening operations at least once.
7. A leather material treated with ash alkali obtained according to the leather ash alkali treatment method according to any one of claims 1 to 6.
8. Use of the leather ash alkali treatment method according to any one of claims 1 to 6 in improving the leather yield of leather.
Citation Information
Patent Citations
Method for carrying out unhairing and liming treatment without dust and akali sulphide during buffalo hide tanning
CN101445843A
Method for increasing leather area yield
CN102827967A
Processing method for goat skin for clothing
CN108660260A
Tannery waste liquid step-by-step recycling process having improved effect