Electric furnace smelting process with high molten iron ratio, high-purity steel smelting method and wire rod preparation method

Through the electric furnace high-speed iron water ratio smelting process and vacuum refining technology, combined with the use of lime, fluorite, and calcium silicate synthetic slag, the problems of copper-clad steel wire conductivity and pulling performance are solved, and the smelting of high-purity steel is achieved and The preparation of high-conductivity copper-clad steel wire significantly improves the overall performance of copper-clad steel wire.

CN118879965APending Publication Date: 2024-11-01INST OF RES OF IRON & STEEL JIANGSU PROVINCE +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410968905.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The prior art is difficult to effectively control the conductivity and drawing properties of copper-clad steel wire, resulting in high content of impurities in steel, affecting the high purity and mechanical properties of copper-clad steel wire.

Method used

Using the electric furnace high-speed iron water ratio smelting process, combined with the double slag plus furnace slag washing method, the P, S, O, N and other impurities in the molten steel are controlled through the use of high-quality scrap steel and the synthetic slag of lime, fluorite, and calcium aluminosilicate. The content, combined with vacuum refining and LF refining, realize the smelting of high-purity steel, and prepare high-conductivity copper-clad steel wire strips through high-line rolling and cold-controlled processes.

Benefits of technology

The conductivity and drawing performance of copper-clad steel wire is significantly improved, the drawing and breaking rate of the coil strip is reduced, the comprehensive control of impurity elements is achieved, and the overall performance of copper-clad steel wire is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879965A_ABST
    Figure CN118879965A_ABST
Patent Text Reader

Abstract

The invention relates to an electric furnace high molten iron ratio smelting process, a high-purity steel smelting method and a wire rod preparation method, when the price of molten iron is in the market price valley, through the design of molten iron pre-desulfurization, electric furnace high molten iron ratio smelting and LF refining in the whole smelting process, on the basis that the performance is ensured, the high purity steel is obtained; and the contents of alloy elements and impurity elements are reduced to the greatest extent. Through the design of vacuum refining, accurate control over the types of the inclusions is achieved, the inclusions in the molten steel are greatly removed, and the number and size of the inclusions are reduced. The continuous casting process parameters are optimized, the surface quality and the internal quality of a casting blank are controlled, the casting blank with the low defect rate is obtained, meanwhile, the surface quality and the internal quality of the steel wire rod are strictly controlled, the rolling process is improved, the strength of the steel wire rod is reduced, the steel wire rod is easy to draw, and the steel wire rod which is good in drawing performance and not prone to being broken is comprehensively obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an electric furnace high iron to water ratio smelting process, a high purity steel smelting method and a wire rod preparation method, belonging to steel smelting technology. Background Art

[0002] Copper clad steel wire refers to a composite wire with copper wrapped around steel wire, that is, a copper layer wrapped around the outer surface of the steel wire. It uses the skin effect of low-voltage high-frequency signals to travel along the surface in the high-frequency area, so as long as the thickness of the copper layer reaches a certain range, the signal of a certain frequency band can be guaranteed to be transmitted. Copper clad steel wire, as a representative of high conduction efficiency, low cost, high strength, corrosion resistance and wear resistance, has been widely used in telecommunications, electronics, utilities, military and other fields.

[0003] The primary indicator for measuring the quality of copper-clad steel wire is electrical conductivity, followed by the low wire breakage rate of the copper-clad steel wire wire. For electrical conductivity, when the electrical conductivity of the copper layer remains constant, the higher the electrical conductivity of the steel wire, the higher the electrical conductivity of the copper-clad steel wire; for the low wire breakage rate, it is also necessary to ensure the good drawing performance of the steel wire. The method to improve the electrical conductivity and high drawing performance of the steel wire is to reduce the content of impurity elements in the steel. Through the introduction of relevant literature and the application test of electrical conductivity of actual products, it is found that the fewer impurity elements in the steel material, the higher the electrical conductivity, especially the highest electrical conductivity of the single substance, and any alloy or impurity will reduce the electrical conductivity. Therefore, it is very necessary to develop a high-cleanliness steel material to be used as the raw material for copper-clad steel wire wire rod.

[0004] The patent with publication number CN106834591B provides a copper-clad steel smelting method, but the method cancels the hot metal desulfurization pretreatment and vacuum refining, and the sulfur content is difficult to control at an ultra-low S level, which increases the content of sulfide inclusions in the steel, reduces the plasticity and toughness of the steel, and has an adverse effect on the mechanical properties of the wire rod; in addition, the method produces high-basicity slag during the LF refining process, and the slag basicity is 8.0-12.0, which is easy to cause high-melting-point brittle inclusions in the steel to exceed the standard, increasing the wire breakage rate of the wire rod drawing, and at the same time, due to the cancellation of KR desulfurization, RH vacuum treatment and other links, the overall control level of S, O, N and inclusions is poor, and high-conductivity copper-clad steel cannot be obtained. The patent with publication number CN111979495B provides a high-conductivity cable steel and production method for making film capacitor leads, but the content of impurity elements such as P, S, Alt, Si, and N is controlled to be high, which is unfavorable for the control of conductivity and drawing performance. In addition, in order to obtain low oxygen content, Alt is controlled between 0.008-0.010%, which will result in Al being the main component in the molten steel. 2 O 3Inclusions are detrimental to the electrical conductivity and drawing processing performance of the wire rod. The heating time in the heating furnace is long, and it is required not to overburn, but no suitable solution is provided. After the ingot is heated, it is stacked and naturally cooled to room temperature, and then heated again for rough rolling. The process is chaotic and the production cost is high. The patent with publication number CN107675068A provides a production method for steel wire rods for ultra-fine copper-clad steel wire, but during the smelting stage, the steel tapping temperature of the converter is extremely high, which is not conducive to dephosphorization and causes great damage to the furnace body. Secondly, a large amount of aluminum shots or 70Ti deoxidation is added after RH decarburization, and the total oxygen is removed to below 15ppm. The residual Al and Ti content in the molten steel is high, and the inclusions are mainly high-melting-point brittle inclusions such as aluminum oxide and titanium oxide, which have a greater impact on the drawing performance. In addition, the content of impurity elements such as P, S, Mn, and N is also relatively high overall, which has a greater impact on conductivity. The patent with publication number CN113073268A provides a copper-clad steel wire rod and its production method, but its Al, Mn, and P contents are generally high, which is not conducive to improving the conductivity (the impurity elements are high). In addition, the wire rod to which it belongs also has cracks with a depth of less than 50 μm, and the surface quality control is not ideal, which has a great impact on the subsequent drawing performance. In addition, a high Al content can reduce the total oxygen content, but the inclusions are mainly Al 2 O 3 , poor castability, or calcium treatment, the calcium treatment process is not conducive to the control of molten steel cleanliness, and has a great impact on the drawing performance and conductivity of wire rods and products.

[0005] It can be seen that the development of high-purity steel is of great significance to obtaining copper-clad steel wire with high conductivity. Summary of the invention

[0006] The present invention provides an electric furnace high iron to water ratio smelting process, a high purity steel smelting method and a wire rod preparation method, so as to improve the conductivity of copper clad steel wire and reduce the wire breakage rate of wire rod drawing.

[0007] The technical solution adopted by the present invention to solve its technical problem is:

[0008] An electric furnace high iron-water ratio smelting process, when the iron price is at a low point in the market, the iron ratio of the selected raw materials is 75-85%, and high-quality scrap steel is used; the electric furnace adopts double slag plus post-furnace slag washing method for smelting;

[0009] The specific steps are as follows: in the initial stage of electric furnace smelting, the electric furnace oxygen lance and the side wall oxygen lance are not powered on, oxygen is blown for smelting, when the blowing is stopped, the slag basicity of the electric furnace is 1.5-2.2, the T.Fe content in the slag is 20-30%, the temperature is 1350-1420°C, the total amount of slag running and slag pouring is 80-90% in the initial stage of electric furnace blowing, and then slag making and blowing are continued, and the slag basicity of the electric furnace is 4.0-6.5 and the T.Fe content is 30-40% after the blowing is completed, 70-80% of the slag is poured first, and then the power is turned on to increase the temperature, and after the temperature reaches at least 1650°C, the electric furnace starts to tap steel, a slide plate is used to block the slag, and the slide plate of the electric furnace tapping hole is closed before tapping and shaking the furnace, and after the molten steel is completely immersed above the slide plate by more than 20cm, the slide plate of the electric furnace tapping hole is opened to tap steel;

[0010] As a further preferred embodiment of the present invention, the carbon content of the steel tapped from the electric furnace is 0.02-0.05%, the oxygen content is 0.055-0.085%, P≤0.01%, and the tapping temperature is ≥1675°C;

[0011] As a further preferred embodiment of the present invention, when the electric furnace is tapping steel, if P≤0.0050%, lime, fluorite and calcium aluminosilicate synthetic slag are added to the ladle when 70-80% of the steel is tapped, and the steel is transported to a vacuum treatment after the tapping is completed;

[0012] As a further preferred embodiment of the present invention, if P≤0.0050%, 3.5-4.5kg / t of lime, 0.5-1.0kg / t of fluorite, and 4.5-6.5kg / t of calcium silicate synthetic slag are added to the ladle to make slag when 70-80% of the steel is tapped, and the ladle bottom blowing flow rate during the tapping process is 600-800NL / min;

[0013] As a further preferred embodiment of the present invention, when the electric furnace is tapping steel, if P>0.0050%, fine lime and iron oxide powder are added to the ladle slag when the electric furnace is tapping 15-25%; the ladle bottom blowing flow rate during the tapping process is 600-800NL / min, and the tapping is completed.

[0014] 800-1000NL / min, after stirring for 3-5 minutes, stop blowing argon and start slag removal, the slag removal rate is ≥90%, the P content of molten steel is ≤0.005%, then add lime, fluorite and calcium aluminosilicate to synthesize slag, and then transport it to LF for refining and heating;

[0015] As a further preferred embodiment of the present invention, if P>0.0050%, when the electric furnace tapping is 15-25%, the amount of fine lime added is 3.5-4.5kg / t, the particle size of 3-8mm accounts for ≥95%, the slag ratio of other particle sizes is <5%, the particle size is less than or equal to 5mm, the CaO content is ≥96%, and other unavoidable impurity components;

[0016] The amount of iron oxide powder added is 1.5-2.5kg / t, the particle size of 3-10mm accounts for ≥90%, the slag ratio of other particle sizes is <10%, the particle size is less than or equal to 15mm, and the Fe oxide accounts for ≥80%;

[0017] The main components of calcium aluminosilicate synthetic slag are CaO 45-55%, Al 2 O 3 20-30%, SiO 2 15-30%, MgO 3-5%, and other inevitable components, including 2CaO·Al 2 O 3 ·SiO 2 Phase proportion ≥80%;

[0018] As a further preferred embodiment of the present invention, in the high-quality scrap steel, the P content is ≤0.018%, S ≤0.008%, Al ≤0.06%, Ti ≤0.01%, Cr ≤0.08%, Mo ≤0.08%, V ≤0.045%, Sn ≤0.05%, and As ≤0.02%;

[0019] A high purity steel smelting method comprises the following steps:

[0020] Step S1: pretreatment of molten iron, sulfur content after desulfurization ≤ 0.001%, slag after desulfurization, slag removal rate ≥ 97%, temperature ≥ 1300°C;

[0021] Step S2: adopting the electric furnace high iron to water ratio smelting process described in claims 1-7; if P≤0.0050% when the electric furnace is tapping steel, the steel is transported to step S4 for vacuum treatment after tapping; if P>0.0050% when the electric furnace is tapping steel, dephosphorization treatment is performed and then the steel is transported to step S3 for LF refining and heating;

[0022] Step S3: LF refining: the molten steel transported after the electric furnace smelting in step S2 is quickly powered on and heated to above 1620°C for LF refining, and then transported to a vacuum furnace for vacuum treatment in step S4;

[0023] Step S4: Vacuum treatment: during vacuum refining, the vacuum furnace working pressure is set to ≤100Pa. After decarburization for 15 minutes, metal aluminum, FeAlCa or calcium aluminate synthetic slag containing metal aluminum is added for deoxidation. The amount of metal aluminum added is M Al =9 / 8(a·M O -m O )M steel , where M Al is the amount of metal aluminum added, kg; M O The oxygen content at the end of vacuum furnace decarburization, %; m O is the target oxygen content of molten steel tapped from a vacuum furnace, %; M steelis the weight of molten steel, kg; a is the oxygen supply coefficient to molten steel considering slag, vacuum tank and ladle wall cold steel slag, 1.35-1.55;

[0024] As a further preferred embodiment of the present invention, in step S1, during the pretreatment of molten iron, the KR station molten iron has C 4.1-4.5%, Si 0.25-0.60%, Mn ≤ 0.35%, P ≤ 0.10%, S ≤ 0.045%, and Fe and other inevitable components, and the temperature is ≥ 1340°C;

[0025] KR enters the station to the processing position, first removes the blast furnace slag, and the slag removal rate is ≥95%;

[0026] As a further preferred embodiment of the present invention, in step S3, the molten steel after the dephosphorization of the slag from the electric furnace is melted in LF refining, and the lime, fluorite slag and calcium aluminosilicate synthetic slag are melted, and a low-carbon steel slag surface deoxidizer is added during the slagging process to control the oxygen content in the molten steel. At the same time, the molten steel is heated to a preset value and then transported to step S4 for vacuum treatment;

[0027] As a further preferred embodiment of the present invention, 0.5-1.0 kg / t of low carbon steel slag surface deoxidizer is added during the slag-making process, and the main components of the slag surface deoxidizer are Al 30-35%, CaO 40-45%, Al 2 O 3 15-20%, SiO 2 ≤5%, and other unavoidable components, control the oxygen content of molten steel to 0.040-0.065%;

[0028] The molten steel is heated to above 1620°C and transported to step S4 for vacuum treatment;

[0029] As a further preferred embodiment of the present invention, in step S4, the vacuum treatment includes RH vacuum treatment, VD or VOD vacuum treatment;

[0030] As a further preferred embodiment of the present invention, when the vacuum treatment method selected is RH vacuum treatment, the specific steps are: after the ladle arrives at the treatment position, vacuum deep decarburization is carried out quickly, and when the C in the molten steel is ≤0.0025%, a deoxidizer is added for deoxidation, and then the net circulation time is ≥8min, the steel is tapped, and the steel is left to stand for more than 10 minutes before the subsequent procedures are carried out;

[0031] As a further preferred embodiment of the present invention, when the vacuum treatment method selected is VD or VOD vacuum treatment, the specific steps are: placing the ladle in the treatment position, connecting the bottom blowing argon, and starting to evacuate after the vacuum ladle cover is sealed, the bottom blowing argon flow rate is set to 400-600NL / min, and after the C in the molten steel is ≤0.0025%, a deoxidizer is added for deoxidation, 0.8-1.4kg / t of low-carbon steel slag surface deoxidizer is added to the slag surface of the ladle, and then the bottom blowing pressure is reduced to 30-80NL / min, stirring for 5-10 minutes, breaking the air, tapping, soft blowing for more than 15 minutes, and performing subsequent procedures;

[0032] A method for preparing a wire rod, wherein the prepared wire rod has high electrical conductivity, specifically comprising the following steps:

[0033] The first step is production preparation. The steel ladles with the first 20 ladle ages are used for desulfurization. Before copper-clad steel smelting, the molten steel from a furnace of boiling steel is used to clean and heat the vacuum chamber, and the tank is continuously circulated for 10-20 minutes. The refining ladle cover, VD or VOD vacuum tank cover, and RH vacuum tank are all cleaned to remove cold steel, slag and other residues. Unused carbon-free steel ladles are prepared. Low-carbon refractory materials and protective slag are prepared for continuous casting.

[0034] The second step is to adopt the whole process steps of the high purity steel smelting method according to claim 6, and after completing vacuum refining, transport to the third step of continuous casting process;

[0035] The third step is continuous casting of large square billets, with a continuous casting section of 300mm×390mm and a strong cooling process;

[0036] The fourth step is to grind the blank. Set the heating furnace temperature and the blanking temperature. Perform magnetic particle inspection after blanking. Grind the entire surface. Perform partial grinding based on the inspection results to ensure that there are no obvious defects on the surface.

[0037] The fifth step is high-speed wire rolling, setting the rolling start temperature and the wire laying temperature, controlling the cooling on the Stelmor controlled cooling line, controlling the Stelmor controlled cooling line fan switch and air volume, and the number of insulation cover switches, performing slow cooling, and controlling the wire rod strength;

[0038] The sixth step is packaging and transportation. The packing line and the wire rod are separated by soft wear-resistant materials, and wide packing tape is used with a width of 3-5cm and a binding pressure of 20-40MPa to avoid scratches on the wire rod during transportation and lifting;

[0039] As a further preferred embodiment of the present invention, in the first step of production preparation, after the ladle is charged with iron into the electric furnace each time, the ladle is hoisted into the cleaning position, and after being turned over, the residue in the ladle is cleaned with a high-pressure air gun, and the nodules at the ladle mouth are cleaned with a bag unpacker;

[0040] The prepared unused carbon-free ladle has a C content of ≤1.5%, a baking time of ≥30 hours, and a temperature of ≥1250°C;

[0041] The prepared low-carbon refractory materials include RH vacuum furnace immersion tube, refractory materials in contact with molten steel in the bottom tank, refractory materials in the working layer of the continuous casting tundish, and refractory materials for three large parts of continuous casting. Among them, the C content of RH vacuum furnace immersion tube, refractory materials in contact with molten steel in the bottom tank, refractory materials in the working layer of the continuous casting tundish, and refractory materials for three large parts of continuous casting is ≤10%;

[0042] The C content of mold slag is ≤2%;

[0043] As a further preferred embodiment of the present invention, in the second step, after the deoxidation of the molten steel is completed, the total oxygen is still maintained within 50 ppm, and it is not necessary to deoxidize it to below 15 ppm;

[0044] As a further preferred embodiment of the present invention, in the third step of continuous casting of large square billets, the superheat of the tundish is controlled at 25-45°C, the tonnage of the initial pouring is ≥20 tons, the weight of the molten steel during normal pouring is ≥35 tons, and the tonnage of the tundish during continuous casting and ladle replacement is ≥30 tons;

[0045] As a further preferred embodiment of the present invention, the continuous casting speed is 0.5-0.8 m / min, ultra-low carbon steel protection slag is used, the crystallizer electromagnetic stirring current is 300-500 A, the frequency is 1.5-4.5 Hz, the crystallizer water volume is 2900-3100 NL / min, the inlet and outlet water temperature difference is ≤10°C, and the secondary cooling water volume is 0.38-0.42 NL / kg;

[0046] As a further preferred embodiment of the present invention, a strong cooling process is adopted with a reduction of 15-20 mm; the reduction is distributed among 6-13 pairs of rollers, and the reductions are set to 0.5-1.0 mm, 1.5-2.0 mm, 3.5-4.0 mm, 4.0-4.5 mm, 4.0-4.5 mm, 2.5-3.5 mm, 1.5-2.5 mm, and 1.0-1.5 mm respectively;

[0047] As a further preferred embodiment of the present invention, in the fourth step of blanking and grinding, the heating furnace temperature is set to 1150-1200°C, the blanking temperature is 1120-1150°C, magnetic particle inspection is performed after blanking, and the surface is fully ground, and the grinding depth is ≥0.5mm;

[0048] As a further preferred embodiment of the present invention, the surface of the ingot is dephosphorized before being opened, and after being cleaned, it is sent to a heating furnace for the first heating. After the first heating is completed, the ingot is opened to obtain a billet, magnetic particle inspection is performed on the billet, and local grinding is performed according to the inspection results to ensure that there are no obvious defects on the surface, and then it is sent to a heating furnace for the second heating to obtain a 140 mm × 140 mm small square billet for preparing wire rods;

[0049] As a further preferred embodiment of the present invention, in the fifth step of high-speed wire rolling, the rolling temperature is set to 980-1000°C, the spinning temperature is 880-920°C, all fans of the Stelmor cooling line are turned off, the roller table entrance speed is controlled at 12-18m / min, the maximum speed is controlled at 24-30m / min, the insulation cover of the first section is fully opened, the insulation cover of the second section is opened by 50%, the insulation covers of the third to sixth sections are all closed, and the insulation covers of each section from the seventh section and thereafter are all opened;

[0050] As a further preferred embodiment of the present invention, the obtained high conductivity copper clad steel wire wire rod has the following chemical compositions by mass percentage: C≤0.0030%, Si≤0.008%, Mn≤0.045%, Alt≤0.004%, P≤0.005%, S≤0.0030%, TO≤0.006%, N≤0.0030%, H≤0.00015%, Ti≤0.0008%, Cr≤0.015%, Mo≤0.006%, V≤0.01%, Sn≤0.015%, As≤0.008%, and the rest is Fe and other inevitable impurity components;

[0051] As a further preferred embodiment of the present invention, in the wire rod, the maximum inclusion size is ≤12 μm, the brittle inclusion is ≤5 μm, and the wire rod tensile strength is ≤260 MPa;

[0052] The wire breakage rate of wire rod drawing is ≤0.15 times / ton, and the electrical conductivity is ≥16.9%.

[0053] Through the above technical solution, compared with the prior art, the present invention has the following beneficial effects:

[0054] 1. The electric furnace high iron-to-water ratio smelting process provided by the present invention fully considers the advantage of low difficulty of dephosphorization in electric furnace smelting, and combines the smelting method with high iron-to-water ratio under the premise of low molten iron price, and achieves the purpose of controlling nitrogen content or impurity alloy element content at the same time;

[0055] 2. The high-purity steel smelting method provided by the present invention, through the design of the whole smelting process, first controls the content of conventional alloying elements such as Al, Si, Mn, Ti, and at the same time greatly reduces the content of impurity elements such as C, P, S, O, and N, and further reduces harmful elements such as Cr, Mo, V, Sn, and As by controlling the types and components of molten iron, scrap steel, and deoxidizer, thereby achieving comprehensive control of impurity elements and strictly controlling the number of inclusions, which can significantly improve the conductivity of copper-clad steel; at the same time, the size of inclusions is controlled, so that the drawing performance is also significantly improved;

[0056] 4. The wire rod preparation method provided by the present invention controls the quality of the billet and obtains a low defect rate ingot based on the high iron-water ratio smelting process of the electric furnace and the high purity steel smelting method. In the billet rolling process, the intermediate billet is provided with good surface quality through surface flaw detection, grinding and other measures; in the finishing rolling and controlled cooling stage, a slow cooling process is adopted to obtain a low-strength wire rod and promote the drawing performance of the wire rod. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0058] Figure 1 It is an overall flow chart of the wire rod preparation method provided by the present invention. DETAILED DESCRIPTION

[0059] The present invention will now be described in further detail with reference to the accompanying drawings. The specific dimensions used in this embodiment are only for illustrating the technical solution and do not limit the protection scope of the present invention.

[0060] As described in the background technology, in order to obtain a higher conductivity, copper-clad steel wire needs to strictly control the content of conventional alloying elements (C, Si, Mn, Al), and at the same time, the impurity elements (P, S, TO, N; impurity alloying elements Ti, Cr, Mo, V, Sn, As) are fully controlled, and the content is controlled to an extremely low level, which is very difficult. The existing technology generally uses one or more of the conventional alloying elements to achieve deoxidation, which can control oxygen at a lower level, but will sacrifice the inclusion control effect, and the content of the alloying elements used for deoxidation is high; in addition, the impurity elements require different control process technologies, such as electric furnace deep dephosphorization technology, KR deep desulfurization and scrap steel and auxiliary materials control back sulfur technology, scrap steel and auxiliary materials and other impurity element control technology, etc., and it is difficult to control the existing conventional technology at the same time.

[0061] Among the above-mentioned elements, although P can increase the strength and hardness of steel, it causes a significant decrease in plasticity and impact toughness. Especially at low temperatures, it makes steel significantly brittle, a phenomenon called "cold brittleness". Cold brittleness deteriorates the cold working and weldability of steel. The higher the phosphorus content, the greater the cold brittleness. Phosphorus can also increase the specific resistivity of steel, so the phosphorus content in steel is strictly controlled. Taking into account the difficulty of dephosphorization, the present application has been found after several research tests and combined with actual production that when the price of molten iron is at the bottom of the market price, the phosphorus content in molten steel can be first reduced by smelting with a high iron-to-water ratio in an electric furnace (electric furnace dephosphorization is relatively simple, and the tapping temperature is higher, and electrodes can be used to heat the molten steel after dephosphorization). The high iron-water ratio smelting in the electric furnace can also control the N content or the content of some impurity alloy elements. This is because the effect of N on the performance of steel is similar to that of carbon and phosphorus. With the increase of nitrogen content, the strength of steel can be significantly improved, and the plasticity, especially toughness, is significantly reduced, the weldability is deteriorated, and the cold brittleness is aggravated; at the same time, the aging tendency, cold brittleness and hot brittleness are increased, and the welding performance and cold bending performance of steel are damaged. Therefore, the nitrogen content in steel should be reduced and limited as much as possible. C is the main element second only to iron in general steel, which directly affects the strength, plasticity, toughness and welding performance of steel. With the increase of carbon content, the welding performance of steel deteriorates, the cold brittleness and aging sensitivity increase, the atmospheric corrosion resistance decreases, and the conductivity also decreases significantly. Therefore, oxygen decarburization is carried out at the same time as dephosphorization in the electric furnace to significantly reduce the carbon content.

[0062] Regarding the specific smelting process of high iron-water ratio in electric furnace, the proportion of hot metal in the selected raw materials is 75-85%, and high-quality scrap steel is used; the high-quality scrap steel here must control the alloy elements in the scrap steel elements at a low level, so as to remove the P, Al, Ti, and Cr content in the molten steel during electric furnace smelting; at the same time, reduce the content of Mo and other elements that are not easy to oxidize, so as to avoid their inability to be oxidized and removed during electric furnace smelting. Therefore, the selected high-quality scrap steel has a P content of ≤0.018%, S ≤0.008%, Al ≤0.06%, Ti ≤0.01%, Cr ≤0.08%, Mo ≤0.03%, V ≤0.045%, Sn ≤0.05%, and As ≤0.02%.

[0063] The electric furnace adopts double slag plus post-furnace slag washing method for smelting; the electric furnace is not powered on at the initial stage of smelting, and oxygen is blown by the furnace door oxygen lance and the side wall oxygen lance for smelting. When the blowing is stopped, the slag basicity of the electric furnace is 1.5-2.2, the T.Fe content in the slag is 20-30%, and the temperature is 1350-1420°C. The total amount of slag running and slag pouring is 80-90% at the initial stage of electric furnace blowing, and then slag making and blowing are continued. At the end of blowing, the slag basicity of the electric furnace is 4.0-6.5, and the T.Fe content is 30-40%. First, 70-80% of the slag is poured, and then the power is turned on to increase the temperature. After the temperature reaches at least 1650°C, the electric furnace starts to tap steel, and a slide plate is used to block the slag. Before tapping the steel, the slide plate of the electric furnace tapping hole is closed. After the molten steel is completely immersed above the slide plate by more than 20 cm, the slide plate of the electric furnace tapping hole is opened to tap steel.

[0064] After this step, the carbon content of the steel tapped from the electric furnace is 0.02-0.05%, the oxygen content is 0.050-0.085%, P≤0.01%, and the tapping temperature is ≥1675°C.

[0065] When the electric furnace is tapping steel, whether to carry out dephosphorization treatment is determined according to the specific phosphorus content. If P≤0.0050%, 3.5-4.5kg / t of lime, 0.5-1.0kg / t of fluorite and 4.5-6.5kg / t of calcium silicate synthetic slag are added to the ladle to make slag when 70-80% of the steel is tapped. The bottom blowing flow rate of the ladle during the tapping process is 600-800NL / min. After the tapping is completed, the steel is transported to vacuum treatment.

[0066] When P>0.0050%, dephosphorization treatment is required. At this time, fine lime and iron oxide powder are added to the ladle slag when 15-25% of the electric furnace is tapped. The ladle bottom blowing flow rate during the tapping process is 600-800NL / min, and 800-1000NL / min after the tapping is completed. After stirring for 3-5 minutes, the bottom blowing of argon is stopped and slag removal is started. The slag removal rate is ≥90%, and the P content of the molten steel is ≤0.005%. Then, lime, fluorite and calcium aluminosilicate are added to synthesize the slag, and then it is transported to LF for refining and heating. Among them, the amount of fine lime added is 3.5-4.5kg / t, the particle size of 3-8mm accounts for ≥95%, the slag ratio of other particle sizes is <5%, the particle size is less than or equal to 5mm, the CaO content is ≥96%, and other unavoidable impurities; the amount of iron oxide powder added is 1.5-2.5kg / t, the particle size of 3-10mm accounts for ≥90%, the slag ratio of other particle sizes is <10%, the particle size is less than or equal to 15mm, and the Fe oxide accounts for ≥80%; the main components of calcium silicate synthetic slag are CaO45-55%, Al 2 O 3 20-30%, SiO 2 15-30%, MgO 3-5%, and other inevitable components, including 2CaO·Al 2 O 3 ·SiO 2 Phase ratio ≥80%.

[0067] Based on the smelting process of high iron-to-water ratio in an electric furnace, this application also designs a high-purity steel smelting method. Through the design of the process flow, the design of the process control technology and the control of the raw material conditions, it is able to better achieve the control level of ultra-low content of various elements. Compared with the existing technology, the control is more comprehensive, the content is lower and the effect is better.

[0068] The high purity steel smelting method specifically comprises the following steps:

[0069] Step S1: pretreatment of molten iron. During pretreatment of molten iron, the molten iron entering the KR station contains 4.1-4.5% C, 0.25-0.60% Si, ≤0.35% Mn, ≤0.10% P, ≤0.045% S, and Fe and other inevitable components, with a temperature ≥1340°C. The KR enters the treatment position and first removes the blast furnace slag, with a slag removal rate ≥95%.

[0070] After desulfurization, the S content is ≤0.001%, the slag after desulfurization is scraped off, the slag scraping rate is ≥97%, and the temperature is ≥1300℃; here, the S in the molten iron is removed to an extremely low level, the desulfurization slag is quickly scraped off, and the S element is taken away.

[0071] Step S2: adopt the electric furnace high iron-water ratio smelting process to remove the P content in the molten steel to an extremely low level; if P≤0.0070% when the electric furnace is tapping, the steel tapping is completed and transported to step S4 for vacuum treatment. If it cannot be removed when the electric furnace is tapping, dephosphorization is continued during the steel tapping process to ensure that the P content meets the standard, that is, if P>0.0070%, after dephosphorization treatment, it is transported to step S3 for LF refining and heating. While dephosphorizing, the electric furnace also carries out oxygen blowing and decarburization to remove the C content to about 0.02-0.05% of water, and then the electric furnace boils and taps steel. The molten steel has strong oxidizability, which can reduce the absorption of N from the air during the steel tapping process.

[0072] In the electric furnace high iron to water ratio smelting process, when the molten iron after pretreatment is added to the electric furnace for smelting, it is mixed with low-sulfur scrap steel, lime and other slag-making materials to prevent the molten steel from increasing in sulfur and obtain ultra-low S molten steel.

[0073] Step S3: LF refining: the molten steel transported after the electric furnace smelting in step S2 is quickly powered on and heated to above 1620°C for LF refining, and then transported to a vacuum furnace for vacuum treatment in step S4;

[0074] The molten steel after the dephosphorization of the slag from the electric furnace is melted in the LF refining to melt the lime, fluorite and calcium silicate synthetic slag. During the slag melting process, 0.5-1.0kg / t low carbon steel slag surface deoxidizer is added. The main components of the slag surface deoxidizer are Al 30-35%, CaO40-45%, Al 2 O 3 15-20%, SiO2 ≤5%, and other inevitable components, the oxygen content of the molten steel is controlled to be 0.040-0.065%, and the temperature of the molten steel is raised to above 1620°C and transported to step S4 for vacuum treatment.

[0075] Step S4: Vacuum treatment: during vacuum refining, the vacuum furnace working pressure is set to ≤100Pa. After decarburization for 15 minutes, metal aluminum, FeAlCa or calcium aluminate synthetic slag containing metal aluminum is added for deoxidation. The amount of metal aluminum added is M Al =9 / 8(a·M O -m O )M steel , where M Al is the amount of metal aluminum added, kg; M O The oxygen content at the end of vacuum furnace decarburization, %; m O is the target oxygen content of molten steel tapped from a vacuum furnace, %; M steel is the weight of molten steel, kg; a is the oxygen supply coefficient to the molten steel considering slag, vacuum tank and ladle wall cold slag, 1.35-1.55.

[0076] Another advantage of using the electric furnace high iron-to-water ratio process is that the vacuum treatment after the electric furnace smelting can be RH vacuum treatment, VD or VOD vacuum treatment. Since the electric furnace is powered on, the N content in the molten steel is high, and vacuum treatment must be matched to remove the nitrogen element to the target content. A variety of vacuum treatment methods can be used, making the process flow more selective.

[0077] When the selected vacuum treatment method is RH vacuum treatment, the specific steps are: after the ladle arrives at the treatment position, it is quickly vacuumed for deep decarburization, and when the C in the molten steel is ≤0.0025%, a deoxidizer is added for deoxidation, and then the net circulation time is ≥8min, the air is broken and the steel is tapped, and it is left to stand for more than 10 minutes before the subsequent procedures are carried out.

[0078] When the selected vacuum treatment method is VD or VOD vacuum treatment, the specific steps are: place the ladle in the treatment position, connect the bottom blowing argon, start vacuuming after the vacuum ladle cover is sealed, set the bottom blowing argon flow rate to 400-600NL / min, and after the C in the molten steel is ≤0.0025%, add deoxidizer for deoxidation, add 0.8-1.4kg / t of low-carbon steel slag surface deoxidizer to the slag surface of the ladle, and then reduce the bottom blowing pressure to 30-80NL / min, stir for 5-10 minutes, break the air, tap the steel, soft blow for more than 15 minutes, and proceed with subsequent procedures.

[0079] The combination of the high iron-water ratio smelting process in the electric furnace, LF refining and vacuum treatment can also control the content of many other elements, such as TO content. O is a harmful element in steel. It naturally enters the steel during the decarburization process of steelmaking. The content of alloy elements in copper-clad steel is very low, and oxygen is difficult to remove. During the solidification of molten steel, oxygen and carbon in the solution react to generate CO, or oxygen overflows, which can cause bubble defects. In addition to dissolved oxygen, oxygen in steel mainly exists in the form of FeO, MnO, SiO 2 、Al 2 O 3 The presence of inclusions such as Al and Al reduces the strength and plasticity of steel. In particular, it has a serious impact on fatigue strength and impact toughness. During the electric furnace steel-making and LF refining process, the slag is modified to control the oxygen content and temperature of the molten steel slag, and then C is used for deoxidation under vacuum. After removing most of the oxygen, an appropriate amount of aluminum-containing alloy is added. The amount of addition is controlled well, which can not only remove the oxygen content of the molten steel, but also prevent the Al content in the molten steel from being too high. The main role of Al in steel is to refine the grains and fix the nitrogen in the steel, thereby significantly improving the impact toughness of the steel and reducing the cold brittleness tendency and aging tendency. Al is an important deoxidizing element that can significantly reduce the oxygen content in steel. At the same time, Al can also fix the free oxygen and free nitrogen in the steel, which can prevent the steel wire from aging embrittlement during the wire drawing process. However, too high an Al content will reduce the electrical conductivity. The Ti element is oxidized by the oxidizing atmosphere of the electric furnace, and titanium oxide enters the slag. Then the slag is controlled well during the steel-making process to avoid bringing Ti into the molten steel.

[0080] In all the above steps, by controlling the content of high-quality scrap steel, alloys, lime and other slag materials, the purpose of controlling the content of other impurity alloy elements in molten steel can be achieved. Other elements are impurities, which will not only reduce the conductivity, but also reduce the plasticity or toughness of the wire rod, improve the tensile strength of the wire rod, and are not conducive to subsequent drawing and finished steel wire production. Their content should be reduced as much as possible under the conditions of preparation to meet the high conductivity requirements and take into account the cost. Through the design of the above-mentioned high-purity steel smelting method, other impurity elements can be controlled within the following ranges: Ti≤0.0006%, Cr≤0.01%, Mo≤0.005%, V≤0.006%, Sn≤0.01%, arsenic As≤0.008%, and the rest are Fe and other inevitable impurity components.

[0081] Finally, the finished product, i.e., the copper-clad steel wire wire rod, should have high conductivity and good drawing performance. The internal quality and surface quality of the wire rod will affect the subsequent drawing performance, so it needs to be produced through corresponding processes. Therefore, the present application provides a wire rod preparation method. Figure 1 As shown, the specific steps include:

[0082] The first step is production preparation. The steel ladles with the first 20 ladle ages are used for desulfurization treatment. After the steel ladles are added to the electric furnace each time, the steel ladles are hoisted into the cleaning position, and the residues in the steel ladles are cleaned with a high-pressure air gun after turning over, and the nodules at the ladle mouth are cleaned with a bag unpacker. Before copper-clad steel smelting, the steel molten steel from a furnace of boiling steel is used for cleaning and heating the vacuum chamber, and the treatment is continuously circulated for 10-20 minutes. The refining ladle cover, VD or VOD vacuum tank cover, and RH vacuum tank are all cleaned, and there is no cold steel, slag and other residues. Unused carbon-free steel ladles are prepared, with a C content of ≤1.5%, a baking time of ≥30 hours, and a temperature of ≥1250℃.

[0083] Prepare low-carbon refractory materials, including RH vacuum furnace dipping tube, refractory materials in contact with molten steel in the bottom trough, refractory materials in the working layer of the continuous casting tundish, and refractory materials for three major parts of continuous casting. Among them, the C content of RH vacuum furnace dipping tube, refractory materials in contact with molten steel in the bottom trough is ≤1%, the C content of refractory materials in the working layer of the continuous casting tundish is ≤1%, and the C content of refractory materials for the three major parts of continuous casting is ≤10%; at the same time, select carbon-free or low-carbon refractory materials to reduce refractory erosion during RH to continuous casting process, reduce foreign large-sized inclusions, comprehensively obtain high-purity molten steel, and further improve conductivity.

[0084] Prepare protective slag with C content ≤ 2% for continuous casting process.

[0085] The second step is to adopt the whole process steps of the high-purity steel smelting method, complete vacuum refining, and then transport to the third step of continuous casting process; it should be noted here that in order to obtain high-conductivity copper-clad steel, various elements in the steel are strictly controlled. After the vacuum deep decarburization is completed, there is a large amount of oxygen content in the molten steel. In order to control the content of deoxidizing elements at a low level, the total oxygen in the molten steel is still maintained within 50ppm after the deoxidation of the molten steel is completed. It is not suitable to remove it to below 15ppm, because removing the oxygen content too low will lead to more inclusions produced by the deoxidizing elements. In addition, only strong deoxidizing elements such as Al, Ca, and Mg can remove the oxygen content of the molten steel while controlling their own content to be extremely low. Alloy elements such as Si and Mn can remove the oxygen content of the molten steel to below 50ppm. The high content of dissolved Si and Mn in the molten steel is not conducive to improving the conductivity.

[0086] The third step is continuous casting of large square billets, with a continuous casting section of 300mm×390mm, the superheat of the tundish controlled at 25-45℃, the tonnage of the opening pouring ≥20 tons, the weight of the molten steel during normal pouring ≥35 tons, the tonnage of the tundish during continuous casting and changing the ladle ≥30 tons, the electromagnetic stirring current of the crystallizer is 300-500A, the frequency is 1.5-4.5HZ, the strong cooling process is used, the reduction is 18-22mm; the continuous casting speed is 0.5-0.8m / min, and ultra-low carbon steel is used. Slag protection, crystallizer water volume 2900-3100NL / min, inlet and outlet water temperature difference ≤10℃, secondary cooling water volume 0.38-0.42NL / kg; the pressure is distributed on 6-13 pairs of rollers, and the pressure reduction is set to 0.5-1.0mm, 1.5-2.0mm, 3.5-4.0mm, 4.0-4.5mm, 4.0-4.5mm, 2.5-3.5mm, 1.5-2.5mm, 1.0-1.5mm respectively.

[0087] Since molten steel contains a certain amount of oxygen, a small amount of small bubbles will be formed in the ingot during the continuous casting cooling process. Therefore, continuous casting adopts a high superheat and strong cooling process to promote the overflow of bubbles and ensure the ingot shape. It is combined with a precise distribution of large pressure reduction technology to control the ingot porosity and center quality, etc., to obtain ingots with low defect rate.

[0088] The fourth step is to grind the billet. Set the heating furnace temperature to 1150-1200℃ and the billet opening temperature to 1120-1150℃. Dephosphorize the surface of the billet before billet opening. After cleaning, send it to the heating furnace for the first heating. The heating furnace is in the furnace for 150-180 minutes. After billet opening, a 140mm×140mm billet is obtained. After billet opening, magnetic particle inspection is performed, and the surface is fully ground. The grinding depth is ≥0.5mm. According to the inspection results, local grinding is performed to ensure that there are no obvious defects on the surface. Send it to the heating furnace for the second heating to obtain a small square billet for preparing wire rods. Surface cleaning and billet opening and grinding can improve the surface quality of the intermediate billet and prevent foreign matter such as oxide scale from being pressed into the subsequent rolling process to affect the surface quality.

[0089] The fifth step is high-speed wire rolling. The rolling start temperature is set at 980-1000°C and the wire laying temperature is set at 880-920°C. Controlled cooling is performed on the Stelmor controlled cooling line. The fan switch and air volume of the Stelmor controlled cooling line and the number of insulation cover switches are controlled to perform slow cooling and control the strength of the wire rod. Specifically, controlled cooling is performed on the Stelmor controlled cooling line. The inlet speed, maximum speed and coordination of the fan and insulation cover are controlled. All fans are closed for slow cooling. The inlet speed of the roller table is controlled at 12-18m / min and the maximum speed is controlled at 24-30m / min. The insulation covers of the first section are all opened and 50% of the insulation covers of the second section are opened. The wire laying is controlled to enter the third to sixth sections to reach the phase change temperature. The insulation covers of the third to sixth sections are all closed. In order to ensure the phase change temperature during the phase change of the steel and fully change the phase, the insulation covers of each section from the seventh section and thereafter are all opened because the phase change of the steel has ended at this time. In order to ensure that the wire rod does not roll randomly, the wire rod should be appropriately cooled after the phase change.

[0090] The sixth step is packaging and transportation. The baling line and the wire rod are separated by soft wear-resistant materials, and wide packing tape is used with a width of 3-5cm and a binding pressure of 20-40MPa to avoid scratches on the wire rod during transportation and lifting.

[0091] The high-conductivity copper-clad steel wire wire obtained at last has a chemical composition by mass percentage including: C≤0.0030%, Si≤0.008%, Mn≤0.045%, Alt≤0.004%, P≤0.005%, S≤0.0030%, TO≤0.006%, N≤0.0030%, H≤0.00015%, Ti≤0.0008%, Cr≤0.015%, Mo≤0.006%, V≤0.01%, Sn≤0.015%, As≤0.008%, and the rest is Fe and other unavoidable impurity components. The above is a specific description of an electric furnace high iron water ratio smelting process, a high purity steel smelting method and a wire rod preparation method provided in this application. Next, several embodiments of preparing wire rods after implementing the wire rod preparation method provided above are introduced respectively. The embodiments are mainly provided in the form of specific parameters running through the preparation method.

[0092] Embodiment 1-6:

[0093] After production preparation, the molten iron is pretreated and deep desulfurized. The sulfur element in the molten iron forms desulfurization slag. The S element can be removed by simply scraping off the desulfurization slag. The specific values ​​of the slag scraping rate, the S content of the molten iron after desulfurization, and the tapping temperature are shown in Table 1.

[0094] Table 1

[0095]

[0096] In this step, the KR incoming hot metal contains C 4.1-4.5%, Si 0.25-0.60%, Mn≤0.35%, P≤0.10%, S≤0.045%, and Fe and other unavoidable components, and the temperature is ≥1340°C;

[0097] The molten iron after desulfurization slag removal is added to the electric furnace, and the electric furnace high iron to water ratio smelting process is adopted. High-quality scrap steel is used here; combined with the proportion of molten iron in the selected raw materials, the content of each element selected in the high-quality scrap steel is shown in Table 2.

[0098] Table 2, molten iron ratio and mass fraction of each element in scrap steel, %

[0099]

[0100] The electric furnace adopts double slag plus post-furnace slag washing method for smelting operation. Table 3 shows the slag basicity, T.Fe content in the slag, temperature and total amount of slag dumping when the electric furnace is stopped at the initial stage of smelting.

[0101] Table 3

[0102] Serial number Slag basicity T.Fe content, % Temperature, °C Slag discharge rate, % Example 1 1.6 25.6 1350 86 Example 2 2.1 21.8 1378 83 Example 3 2.2 30.0 1397 90 Example 4 1.5 27.5 1420 85 Example 5 1.9 29.2 1386 80 Example 6 2.0 20.0 1412 84

[0103] Continue slag making and blowing. The slag basicity, T.Fe content, slag pouring rate and temperature of the electric furnace when steel is tapped are shown in Table 4.

[0104] Serial number Slag basicity T.Fe content, % Slag discharge rate, % Steel tapping temperature, ℃ Example 1 5.6 35.0 75 1680 Example 2 6.5 32.5 77 1665 Example 3 4.0 30.0 70 1672 Example 4 5.0 38.6 73 1650 Example 5 4.5 40.0 75 1658 Example 6 5.9 36.1 80 1675

[0105] When the electric furnace starts to tap steel, use a slide plate to block slag. Close the slide plate of the electric furnace tapping hole before tapping steel and open the slide plate to tap steel after the molten steel is completely submerged more than 20 cm above the slide plate.

[0106] In this step, the smelting process with high iron-water ratio removes the P content in the molten steel to an extremely low level; if P≤0.0050% when the electric furnace is tapping, the steel is transported to vacuum treatment after tapping. In the preferred embodiment here, P>0.0050% when the electric furnace is tapping is provided as an example, and dephosphorization is continued during the tapping process to ensure that the P content meets the standard. Specifically, if the steel tapping P in Examples 1 to 6 is greater than 0.0050%, 4.2 kg / t of fine lime is added to the ladle slag when the electric furnace taps 15-25%, with a particle size of 3-8 mm accounting for 97% and a CaO content of 97.3%; 2.1 kg / t of iron oxide powder is added, with a particle size of 3-10 mm accounting for 94%, and Fe oxide accounting for 88%; during the steel tapping process, the ladle bottom blowing flow rate is 650 NL / min, which is set to 860 NL / min after the steel tapping is completed. After stirring for 4.5 minutes, the bottom blowing of argon is stopped, and slag removal is started, with a slag removal rate of 95%, and a P content of molten steel ≤ 0.005%; calcium aluminosilicate synthetic slag is added, and 2CaO·Al in the calcium aluminosilicate synthetic slag is 0.005%. 2 O3 ·SiO 2 The proportion is 86%.

[0107] The molten steel transported after electric furnace smelting is melted in LF refining to melt lime, fluorite slag and calcium aluminosilicate synthetic slag. The main components of the low-carbon steel slag surface deoxidizer added during the slagging process are shown in Table 5.

[0108] Table 5 Content of each component, wt%

[0109]

[0110] The content of deoxidizer added to the surface of low carbon steel slag during the slagging process is 0.5-1.0kg / t. At the same time, the temperature of the molten steel rises to above 1620℃ and is transported for vacuum treatment.

[0111] The high iron-water ratio process of the electric furnace has an advantage, that is, the vacuum treatment after the electric furnace smelting can be RH vacuum treatment, VD or VOD vacuum treatment. In Examples 1 to 6, RH vacuum treatment is the preferred method. When performing RH vacuum treatment, the oxygen content of the RH incoming molten steel is 0.04-0.065%, the oxygen content of the molten steel after RH decarburization is 0.025-0.043%, and the target oxygen content of the RH outgoing molten steel is 0.0050%. The various parameters set are shown in Table 6, including the working pressure of the vacuum chamber, the amount of metal aluminum added, and the carbon content in the molten steel after vacuum deep decarburization treatment, etc.

[0112] Table 6

[0113]

[0114] Next is the large square billet continuous casting process. The parameters set are shown in Table 7:

[0115] Table 7

[0116]

[0117] After the continuous casting process is completed, Table 8 shows the relevant technical parameters of billet grinding and high-speed wire rolling:

[0118] Table 8

[0119]

[0120] The chemical components of the wire rod obtained by the above preparation method are shown in Table 9:

[0121] Table 9 Element composition content, %

[0122] Serial number C Si Mn Alt P S O Example 1 0.0030 0.0065 0.030 0.0025 0.0035 0.0022 0.0042 Example 2 0.0025 0.0045 0.026 0.0023 0.0041 0.0030 0.0055 Example 3 0.0021 0.0080 0.040 0.0035 0.0022 0.0026 0.0036 Example 4 0.0018 0.0053 0.036 0.0031 0.0050 0.0028 0.0060 Example 5 0.0023 0.0071 0.045 0.0040 0.0046 0.0025 0.0043 Example 6 0.0029 0.0030 0.041 0.0020 0.0037 0.0027 0.0035

[0123] Continued

[0124] Serial number N H Ti Cr Mo V Sn As Example 1 0.0025 0.00012 0.0002 0.008 0.002 0.005 0.007 0.005 Example 2 0.0018 0.00008 0.0005 0.007 0.003 0.007 0.003 0.002 Example 3 0.0023 0.00006 0.0008 0.012 0.006 0.004 0.015 0.003 Example 4 0.0030 0.00015 0.0003 0.009 0.004 0.010 0.008 0.006 Example 5 0.0028 0.00013 0.0004 0.015 0.002 0.008 0.005 0.008 Example 6 0.0024 0.00010 0.0006 0.013 0.005 0.003 0.006 0.004

[0125] As a result, the wire rod has the characteristics shown in Table 10.

[0126] Table 10

[0127]

[0128] It can be seen from the above embodiments that the electrical conductivity of the wire rod prepared by the present application is ≥16.9%. When used to make copper-clad steel wire, the thickness of the surface copper plating layer can be reduced, the production cost of downstream enterprises can be reduced, the size of inclusions in the wire rod is reduced, the number of large-sized inclusions is small, the number of brittle inclusions is small, and the size is small. It is not easy to break the wire during the subsequent wire rod deep processing and drawing process. The wire breakage rate of the wire rod drawing is ≤0.15 times / ton, which significantly reduces the wire breakage rate during the deep processing of the wire rod. Compared with the traditional method, the low-strength wire rod rolling process produces a wire rod with a tensile strength of ≤260MPa, which is easy to draw during the deep processing process, and the surface and internal defects of the wire rod are reduced by large pressing, blanking and grinding, further improving the drawing performance of the wire rod.

[0129] It will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those generally understood by those skilled in the art to which this application belongs. It should also be understood that terms such as those defined in common dictionaries should be understood to have meanings consistent with the meanings in the context of the prior art, and will not be interpreted with idealized or overly formal meanings unless defined as herein.

[0130] The meaning of "and / or" described in this application means that the situations where each exists alone or both exist at the same time are included.

[0131] The term “connection” as used in this application may mean a direct connection between components or an indirect connection between components via other components.

[0132] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. An electric furnace high iron to water ratio smelting process, characterized in that: When the price of hot metal is at the bottom of the market, hot metal accounts for 75-85% of the selected raw materials, and high-quality scrap steel is used; the electric furnace adopts double slag plus post-furnace slag washing method for smelting; The specific steps are as follows: at the initial stage of electric furnace smelting, the electric furnace is not powered on, oxygen lances at the furnace door and side wall are used for oxygen blowing, when the blowing is stopped, the slag basicity of the electric furnace is 1.5-2.2, the T.Fe content in the slag is 20-30%, the temperature is 1350-1420°C, the total amount of slag running and slag pouring is 80-90% at the initial stage of electric furnace blowing, and then slag making and blowing are continued, at the end of blowing, the slag basicity of the electric furnace is 4.0-6.5, the T.Fe content is 30-40%, 70-80% of the slag is poured first, and then the power is turned on to increase the temperature, after the temperature reaches at least 1650°C, the electric furnace starts to tap steel, a slide plate is used to block the slag, the electric furnace tapping hole slide plate is closed before tapping and shaking the furnace, and after the molten steel is completely immersed above the slide plate by more than 20cm, the electric furnace tapping hole slide plate is opened to tap steel.

2. The electric furnace high iron to water ratio smelting process according to claim 1, characterized in that: The carbon content of steel produced by the electric furnace is 0.02-0.05%, the oxygen content is 0.050-0.085%, P≤0.01%, and the steel-producing temperature is ≥1675℃.

3. The electric furnace high iron to water ratio smelting process according to claim 2, characterized in that: When the electric furnace is tapping steel, if P≤0.0050%, lime, fluorite and calcium aluminosilicate synthetic slag are added to the ladle when 70-80% of the steel is tapped, and the slag is transported to vacuum treatment after the tapping is completed.

4. The electric furnace high iron to water ratio smelting process according to claim 3, characterized in that: If P≤0.0050%, add 3.5-4.5kg / t of lime, 0.5-1.0kg / t of fluorite and 4.5-6.5kg / t of calcium silicate synthetic slag into the ladle to make slag when 70-80% of the steel is tapped. The bottom blowing flow rate of the ladle during the tapping process is 600-800NL / min.

5. The electric furnace high iron to water ratio smelting process according to claim 2, characterized in that: When the electric furnace is tapping steel, if P>0.0050%, fine lime and iron oxide powder are added to the ladle slag when the electric furnace tapping is 15-25%; the ladle bottom blowing flow rate during the tapping process is 600-800NL / min, and 800-1000NL / min at the end of tapping. After stirring for 3-5 minutes, the bottom blowing of argon is stopped and slag removal is started. The slag removal rate is ≥90%, and the P content of the molten steel is ≤0.005%. Then, lime, fluorite and calcium aluminosilicate are added to synthesize the slag, and then it is transported to LF for refining and heating.

6. The electric furnace high iron to water ratio smelting process according to claim 5, characterized in that: If P>0.0050%, when the electric furnace tapping is 15-25%, the amount of fine lime added is 3.5-4.5kg / t, the particle size of 3-8mm accounts for ≥95%, the slag ratio of other particle sizes is <5%, the particle size is less than or equal to 5mm, the CaO content is ≥96%, and other unavoidable impurity components; The amount of iron oxide powder added is 1.5-2.5kg / t, the particle size of 3-10mm accounts for ≥90%, the slag ratio of other particle sizes is <10%, the particle size is less than or equal to 15mm, and the Fe oxide accounts for ≥80%; The main components of calcium aluminosilicate synthetic slag are CaO 45-55%, Al2O3 20-30%, SiO2 15-30%, MgO 3-5%, and other inevitable components, among which 2CaO·Al2O3·SiO2 phase accounts for ≥80%.

7. The electric furnace high iron to water ratio smelting process according to claim 1, characterized in that: In the high-quality scrap steel, the content of P is ≤0.018%, S is ≤0.008%, Al is ≤0.06%, Ti is ≤0.01%, Cr is ≤0.08%, Mo is ≤0.03%, V is ≤0.045%, Sn is ≤0.05%, and As is ≤0.02%.

8. A high purity steel smelting method, characterized in that: The following steps are involved: Step S1: pretreatment of molten iron, S content after desulfurization ≤ 0.001%, slag after desulfurization, slag removal rate ≥ 97%, temperature ≥ 1300°C; Step S2: adopting the electric furnace high iron to water ratio smelting process described in claims 1-7; if P≤0.0070% when the electric furnace is tapping steel, the steel is transported to step S4 for vacuum treatment after tapping; if P>0.0070% when the electric furnace is tapping steel, dephosphorization treatment is performed and then transported to step S3 for LF refining and heating; Step S3: LF refining: the molten steel transported after the electric furnace smelting in step S2 is quickly powered on and heated to above 1620°C for LF refining, and then transported to a vacuum furnace for vacuum treatment in step S4; Step S4: Vacuum treatment: during vacuum refining, the vacuum furnace working pressure is set to ≤100Pa. After decarburization for 15 minutes, metal aluminum, FeAlCa or calcium aluminate synthetic slag containing metal aluminum is added for deoxidation. The amount of metal aluminum added is M Al =9 / 8(a·M O -m O )M steel , where M Al is the amount of metal aluminum added, kg; M O The oxygen content at the end of vacuum furnace decarburization, %; m O is the target oxygen content of molten steel tapped from a vacuum furnace, %; M steel is the weight of molten steel, kg; a is the oxygen supply coefficient to the molten steel considering slag, vacuum tank and ladle wall cold slag, 1.35-1.

55.

9. The high purity steel smelting method according to claim 8, characterized in that: In step S1, during the pretreatment of molten iron, the molten iron entering the KR station has C 4.1-4.5%, Si 0.25-0.60%, Mn≤0.35%, P≤0.10%, S≤0.045%, as well as Fe and other inevitable components, and the temperature is ≥1340°C; KR enters the station to the processing position and first removes the blast furnace slag, with the slag removal rate ≥ 95%.

10. The high purity steel smelting method according to claim 8, characterized in that: In step S3, the molten steel after the dephosphorization of the slag from the electric furnace is melted in LF refining to melt the lime, fluorite and calcium aluminosilicate synthetic slag. During the slagging process, a low-carbon steel slag surface deoxidizer is added to control the oxygen content in the molten steel. At the same time, the molten steel is heated to a preset value and then transported to step S4 for vacuum treatment.

11. The high purity steel smelting method according to claim 10, characterized in that: During the slag-melting process, add 0.5-1.0kg / t low-carbon steel slag surface deoxidizer, the main components of the slag surface deoxidizer are Al 30-35%, CaO 40-45%, Al2O315-20%, SiO2≤5%, and other inevitable components to control the oxygen content of the molten steel to 0.040-0.065%; The molten steel is heated to above 1620°C and transported to step S4 for vacuum treatment.

12. The high purity steel smelting method according to claim 8, characterized in that: In step S4, the vacuum treatment includes RH vacuum treatment, VD or VOD vacuum treatment.

13. The high purity steel smelting method according to claim 12, characterized in that: When the selected vacuum treatment method is RH vacuum treatment, the specific steps are: after the ladle arrives at the treatment position, it is quickly vacuumed for deep decarburization, and when the C in the molten steel is ≤0.0025%, a deoxidizer is added for deoxidation, and then the net circulation time is ≥8min, the air is broken and the steel is tapped, and it is left to stand for more than 10 minutes before the subsequent procedures are carried out.

14. The high purity steel smelting method according to claim 12, characterized in that: When the selected vacuum treatment method is VD or VOD vacuum treatment, the specific steps are: place the ladle in the treatment position, turn on the bottom blowing argon, start vacuuming after the vacuum ladle cover is sealed, set the bottom blowing argon flow rate to 400-600NL / min, and after the C in the molten steel is ≤0.0025%, add deoxidizer for deoxidation, add 0.8-1.4kg / t of low-carbon steel slag surface deoxidizer to the slag surface of the ladle, and then reduce the bottom blowing pressure to 30-80NL / min, stir for 5-10 minutes, break the air, tap the steel, soft blow for more than 15 minutes, and proceed with subsequent procedures.

15. A method for preparing a wire rod, wherein the prepared wire rod has high electrical conductivity, characterized in that: The specific steps include: The first step is production preparation. The steel ladles with the first 20 ladle ages are used for desulfurization. Before copper-clad steel smelting, the molten steel from a furnace of boiling steel is used to clean and heat the vacuum chamber, and the tank is continuously circulated for 10-20 minutes. The refining ladle cover, VD or VOD vacuum tank cover, and RH vacuum tank are all cleaned to remove cold steel, slag and other residues. Unused carbon-free steel ladles are prepared. Low-carbon refractory materials and protective slag are prepared for continuous casting. The second step is to adopt the whole process steps of the high purity steel smelting method according to claim 6, and after completing vacuum refining, transport to the third step of continuous casting process; The third step is continuous casting of large square billets, with a continuous casting section of 300mm×390mm and a strong cooling process; The fourth step is to grind the blank. Set the heating furnace temperature and the blanking temperature. Perform magnetic particle inspection after blanking. Grind the entire surface. Perform partial grinding based on the inspection results to ensure that there are no obvious defects on the surface. The fifth step is high-speed wire rolling, setting the rolling start temperature and the wire laying temperature, controlling the cooling on the Stelmor controlled cooling line, controlling the Stelmor controlled cooling line fan switch and air volume, and the number of insulation cover switches, performing slow cooling, and controlling the wire rod strength; The sixth step is packaging and transportation. The baling line and the wire rod are separated by soft wear-resistant materials, and wide packing tape is used with a width of 3-5cm and a binding pressure of 20-40MPa to avoid scratches on the wire rod during transportation and lifting.

16. The method for preparing wire rod according to claim 15, characterized in that: The first step is production preparation. After the ladle is charged with iron into the electric furnace, the ladle is hoisted into the cleaning position, and after turning over, the residue in the ladle is cleaned with a high-pressure air gun, and the nodules at the ladle mouth are cleaned with a bag unpacker. The prepared unused carbon-free ladle has a C content of ≤1.5%, a baking time of ≥30 hours, and a temperature of ≥1250°C; The prepared low-carbon refractory materials include RH vacuum furnace immersion tube, refractory materials in contact with molten steel in the bottom tank, refractory materials in the working layer of the continuous casting tundish, and refractory materials for three large parts of continuous casting. Among them, the C content of RH vacuum furnace immersion tube, refractory materials in contact with molten steel in the bottom tank, refractory materials in the working layer of the continuous casting tundish, and refractory materials for three large parts of continuous casting is ≤10%; The C content of the mold slag is ≤2%.

17. The method for preparing wire rod according to claim 15, characterized in that: In the second step, after the deoxidation of the molten steel is completed, the total oxygen is still maintained within 50ppm, and it is not necessary to deoxidize it to below 15ppm.

18. The method for preparing wire rod according to claim 15, characterized in that: In the third step of continuous casting of large square billets, the superheat of the tundish is controlled at 25-45℃, the tonnage of the initial pouring is ≥20 tons, the weight of the molten steel during normal pouring is ≥35 tons, and the tonnage of the tundish is ≥30 tons during continuous casting and ladle changing.

19. The method for preparing wire rod according to claim 18, characterized in that: The continuous casting speed is 0.5-0.8m / min, ultra-low carbon steel protection slag is used, the crystallizer electromagnetic stirring current is 300-500A, the frequency is 1.5-4.5HZ, the crystallizer water volume is 2900-3100NL / min, the inlet and outlet water temperature difference is ≤10℃, and the secondary cooling water volume is 0.38-0.42NL / kg.

20. The method for preparing wire rod according to claim 19, characterized in that: The strong cooling process is adopted, with a reduction of 15-20mm; the reduction is distributed among 6-13 pairs of rollers, and the reductions are set to 0.5-1.0mm, 1.5-2.0mm, 3.5-4.0mm, 4.0-4.5mm, 4.0-4.5mm, 2.5-3.5mm, 1.5-2.5mm, and 1.0-1.5mm respectively.

21. The method for preparing wire rod according to claim 15, characterized in that: The fourth step is blanking and grinding. Set the heating furnace temperature to 1150-1200℃ and the blanking temperature to 1120-1150℃. After blanking, perform magnetic particle inspection and fully grind the surface. The grinding depth is ≥0.5mm.

22. The method for preparing wire rod according to claim 21, characterized in that: Before opening, the surface of the ingot is dephosphorized, cleaned and sent to a heating furnace for the first heating. After the first heating is completed, the ingot is opened to obtain the ingot, which is subjected to magnetic particle inspection and local grinding according to the inspection results. After ensuring that there are no obvious defects on the surface, it is sent to a heating furnace for the second heating to obtain a small square billet of 140mm×140mm for preparing wire rod.

23. The method for preparing wire rod according to claim 15, characterized in that: For the fifth step of high-speed wire rolling, the starting rolling temperature is set at 980-1000℃, the spinning temperature is 880-920℃, all fans of the Stelmor controlled cooling line are turned off, the roller table entrance speed is controlled at 12-18m / min, the maximum speed is controlled at 24-30m / min, the insulation covers of the first section are all opened, 50% of the insulation covers of the second section are opened, the insulation covers of the third to sixth sections are all closed, and the insulation covers of each section from the seventh section onwards are all opened.

24. The method for preparing wire rod according to claim 15, characterized in that: The obtained high-conductivity copper-clad steel wire wire rod has the following chemical compositions by mass percentage: C≤0.0030%, Si≤0.008%, Mn≤0.045%, Alt≤0.004%, P≤0.005%, S≤0.0030%, O≤0.006%, N≤0.0030%, H≤0.00015%, Ti≤0.0008%, Cr≤0.015%, Mo≤0.006%, V≤0.01%, Sn≤0.015%, As≤0.008%, and the rest are Fe and other inevitable impurity components.

25. The method for preparing wire rod according to claim 24, characterized in that: In the wire rod, the maximum inclusion size is ≤12 μm, the brittle inclusion is ≤5 μm, and the wire rod tensile strength is ≤260 MPa; The wire breakage rate of wire rod drawing is ≤0.15 times / ton, and the electrical conductivity is ≥16.9%.

Citation Information

Cited By

  • Production method of small square billet and wire rod and weaving processing method of wire rod

    CN121874628A