Wire rod for high-strength bridge cable and production method of wire rod

By adopting the high-strength design and advanced smelting technology of 87SiMn coils in the bridge cables, the problem of insufficient strength and plastic toughness of bridge cables in the existing technology is solved, and the strength of the coils above 1400MPa and the level of 2200~2300MPa is achieved. The bridge cable requirements improve hot-dip galvanizing performance and production efficiency.

CN118880169APending Publication Date: 2024-11-01HUNAN VALIN XIANGTAN IRON & STEEL CO LTD
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202410909044.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing steel wires for bridge cables have shortcomings in high strength and plastic toughness, especially in the problem of degradation of torsional performance during hot-dip galvanization during cold drawing processing, and lack of matching component design and advanced cold drawing processing technology.

Method used

Adopting the high-strength design of 87SiMn strips, the chemical composition is C: 0.85-0.92%, Si: 1.2-1.5%, Mn: 0.90-1.0%, Cr: 0.30-0.35%, etc., and it is pretreated by molten iron, converter smelting, LF Refining, VD vacuum furnace treatment, continuous casting and high-speed rolling processes control the content of harmful elements and tissue morphology, and improve the tensile strength and plasticity of steel wires.

Benefits of technology

The coil strength of the above 1400MPa is achieved, meeting the requirements of ultra-high strength bridge cables of 2200~2300MPa, improving the hot-dip galvanizing performance and production efficiency of the steel wire, and reducing costs and environmental impacts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880169A_ABST
    Figure CN118880169A_ABST
Patent Text Reader

Abstract

The invention relates to a wire rod for a high-strength bridge cable and a production method thereof, the wire rod for the high-strength bridge cable is a wire rod 87SiMn, and the wire rod comprises the following chemical components in percentage by weight: 0.85-0.92% of C, 1.2-1.5% of Si, 0.90-1.0% of Mn, 0.30-0.35% of Cr, less than or equal to 0.015% of P, less than or equal to 0.010% of S, less than or equal to 0.10% of Ni, less than or equal to 0.10% of Cu, less than or equal to 0.04% of Al, less than or equal to 0.001% of [O], less than or equal to 0.006% of [N], less than or equal to 0.0100% of Sn, less than or equal to 0.0100% of As and the balance of Fe and inevitable impurities. The invention further discloses a production method of the high-strength steel wire rod for the bridge cable. A reasonable component system and advanced smelting and controlled rolling and controlled cooling processes are adopted, generation of abnormal structures of the wire rod is effectively inhibited, the tensile strength and sorbite rate of the wire rod are improved, the plasticity of the wire rod is improved, waste heat of the wire rod enters a heat preservation vestibule, and online aging is achieved. The strength of the wire rod reaches 1400 MPa or above and is 100 MPa higher than that of common 87B-grade high steel, the sorbite content of the wire rod reaches 95% or above, and the wire rod can be delivered and used after being offline.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel smelting, and in particular relates to a wire rod for high-strength bridge cables and a production method thereof. Background Art

[0002] As bridge construction develops towards crossing the sea, crossing the river, crossing the Greater Bay Area, and crossing the mountains and valleys, the spans of suspension bridges and cable-stayed bridges are getting larger and larger, and the requirements for steel wires for bridge cables are getting higher and higher. The microstructure of steel wires for bridge cables has a double-layer composite structure, which is composed of cementite lamellae and ferrite lamellae spaced apart from each other. The cementite lamellae determine its strength, and the ferrite lamellae determine its plastic toughness. The size of the interlayer spacing between the two is particularly important for its strength-toughness ratio. The original tensile strength of the wire rod and the deformation amount during the cold drawing process jointly determine the final tensile strength of the cold-drawn steel wire. The changes in the microstructure morphology and the accumulated deformation energy during the cold drawing process are the key factors that cause the torsional performance of the steel wire to decrease during the hot-dip galvanizing process. The shortcomings of ultra-high-strength steel wires for bridge cables are mainly the lack of component design and heat treatment technology that matches the higher-strength wire rods, and the lack of advanced cold drawing processing technology to prevent the torsional performance of the steel wire from decreasing during the hot-dip galvanizing process. Summary of the invention

[0003] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art, provide a high-strength wire rod for bridge cables and a production method thereof, increase the strength of the wire rod, improve the plasticity of the wire rod, and ensure the troostitization rate of the wire rod.

[0004] The technical solution adopted by the present invention to solve its technical problem is:

[0005] The wire rod for high-strength bridge cables of the present invention is wire rod 87SiMn, and the chemical composition and weight percentage of the wire rod 87SiMn are: C: 0.85-0.92%, Si: 1.2-1.5%, Mn: 0.90-1.0%, Cr: 0.30-0.35%, P≤0.015%, S≤0.010%, Ni≤0.10%, Cu≤0.10%, Al≤0.04%, [O] (oxygen content in steel)≤0.001%, [N] (nitrogen content in steel)≤0.006%, Sn≤0.0100%, As≤0.0100%, and the rest are Fe and unavoidable impurities.

[0006] The present invention selects special molten iron to control harmful residual elements, and reduces the S content of the molten iron through molten iron pretreatment.

[0007] Furthermore, the strength of 87SiMn wire rod with a diameter of 14mm reaches over 1400MPa.

[0008] Furthermore, the wire rod 87SiMn meets the technical requirements for manufacturing ultra-high strength bridge cables with a single wire specification of Φ5.0mm and a strength level of 2200-2300MPa.

[0009] The production process of high-strength wire rod for bridge cables is: hot metal pretreatment → BOF (BOF refers to converter) → LF refining → VD vacuum furnace treatment → 180*180mm 2 Continuous casting → slow cooling of billet → high-speed wire rolling.

[0010] The production method of the high-strength wire rod for bridge cables of the present invention comprises the following steps:

[0011] (1) Converter smelting: The converter adopts the double slag method, and the steel tapping uses a slide plate to block the slag;

[0012] (2) LF refining: LF refining uses aluminum particles for diffusion deoxidation, the white slag time is kept above 20 minutes, and the slag system adopts a ternary slag system;

[0013] (3) VD vacuum treatment: During the VD vacuum treatment, the vacuum degree is below 67Pa, the time is ≥12 minutes, the hydrogen content in the molten steel is controlled below 1.5ppm, and the superheat of the tundish is controlled at 20-30℃;

[0014] (4) Continuous casting: adopt full-process protection pouring, constant casting speed production, low superheat pouring, use of crystallizer, end electromagnetic stirring, light and heavy pressure reduction technology, and combined with the strong cooling process of water cooling + mist cooling in the secondary cooling zone;

[0015] (5) Rolling: The rolling process adopts a walking beam heating furnace, and the finishing rolling adopts the "8+4" mode, i.e., the finishing rolling unit + the sizing unit rolling. The wire rod size is measured in real time by an online diameter gauge, and the wire rod is cooled by a Stelmor air cooling line and insulated by an insulation corridor.

[0016] Furthermore, the converter adopts the double slag method to effectively reduce the phosphorus content, and the slide plate is used to block the slag during steel discharge to prevent slag from falling from the converter, thereby controlling the purity of the molten steel from the source.

[0017] Furthermore, in the continuous casting process of step (4), 180*180mm 2 The cross-section of the billet production. The crystallizer electromagnetic stirring current is 380-420A (preferably 400A), the frequency is 3.4-3.6Hz (preferably 3.5Hz); the end electromagnetic stirring current is 680-720A (preferably 700A), the frequency is 9-11Hz (preferably 10Hz). The specific water volume is 0.4-0.5L / Kg (preferably 0.45L / Kg), and the total pressure reduction is 20-30mm (preferably 25mm).

[0018] Furthermore, during the continuous casting process of step (4), the casting speed is constant and the casting speed of the continuous casting furnace is controlled at 1-3 m / min (preferably 1.2-1.8 m / min).

[0019] Furthermore, during the continuous casting process of step (4), the superheat is stabilized at 20 to 30°C.

[0020] Furthermore, in step (4), the steel billet after continuous casting is slowly cooled for 24 hours and then hot rolled.

[0021] Step (4) continuous casting operation reduces the columnar crystal area and increases the equiaxed crystal area, prevents the development of columnar crystals, reduces the component segregation of molten steel during solidification, and improves the core and surface quality of the continuously cast billet.

[0022] Furthermore, in step (5), the main process parameters of the rolling are: heating in the heating furnace for one stage at 980-1020°C (preferably 1000°C), heating in the second stage at 1140-1160°C (preferably 1150-1160°C), soaking stage at 1170-1200°C (preferably 1180°C), finishing mill at 860-880°C (preferably 870°C), warp reduction at 880-920°C (preferably 900°C), spinning at 840°C to 860°C; roller speed at 0.6-0.8 m / s (preferably 0.7 m / s); and total heating time in the heating furnace at 120 to 180 min.

[0023] Further, in step (5), the air cooling parameters of the Stelmore air cooling line are: 13-15 (preferably 14) fans, and the air volume of each fan is 180,000-220,000 (preferably 200,000) m 3 / h, wind pressure 2800-3200Pa (preferably 3000Pa).

[0024] Furthermore, in step (5), the process parameters of the insulation corridor are: the temperature entering the insulation corridor is 400-500°C, and the insulation time is more than 120 minutes.

[0025] The wire rod obtained by the invention has a strength of 1400-1460 MPa and is used to produce 2200-2300 MPa ultra-high strength bridge cables.

[0026] The high-strength wire rod for bridge cables and its production method of the present invention use square billet-fired materials to produce Φ14mm-hot-rolled wire rod for bridge cables, mainly using high-carbon, high-silicon and high-manganese component system to improve the strength of the wire rod, improve the plasticity of the wire rod, and use reasonable controlled rolling and controlled cooling process to ensure the sorbitization rate of the wire rod, ensure the strength of the steel wire, and improve the plasticity of the wire rod. The strength of the hot-rolled wire rod reaches 1400-1460MPa, which meets the use requirements of making 2200-2300MPa ultra-high strength bridge cables, and the cost of the square billet-fired materials is low.

[0027] The present invention adopts 180*180mm 2 The square billet and fire material are used to produce 87SiMn hot-rolled wire rod. The base material does not undergo billeting and lead bath / salt bath heat treatment, and the single wire strength can meet the bridge cable requirements of 2200-2300MPa.

[0028] The principle of the present invention is as follows: high Si content can improve the strength of the wire rod, improve the elastic limit and fatigue strength of the steel, and have a certain promoting effect on reducing the spacing between the sorbite lamellae; appropriately increasing the Cr content can greatly improve the strength of the wire rod, and chromium can improve the stability of austenite, shift the C curve to the right, reduce the critical cooling rate, and improve the hardenability of the steel, thereby further reducing the probability of network carbon formation; Mn can improve the strength of the steel without affecting the surface shrinkage of the material; Al can play a role in refining the grains and improving the strength.

[0029] Too high aluminum content will increase costs and production difficulty, while too low aluminum content will not be able to refine the grains.

[0030] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention adopts square billet and one fire material to produce Φ14mm specification 87 grade hot-rolled wire rod, adopts a rationally designed component system, advanced smelting process, and adopts advanced controlled rolling and controlled cooling process, effectively inhibits the generation of abnormal organization of wire rod, improves the plasticity of wire rod, and uses the residual heat of wire rod to enter the insulation corridor to achieve online aging; at the same time, the tensile strength and sorbitization rate of wire rod are improved, and the plasticity of wire rod is improved while ensuring the strength of steel wire. The strength of hot-rolled wire rod reaches more than 1400MPa, which is more than 100Mpa higher than that of ordinary 87B grade high steel, and the sorbitan content of wire rod reaches more than 95%, which meets the use requirements of making 2200-2300MPa ultra-high strength bridge cable. At the same time, the cost of square billet and one fire material is low, the product competitiveness is strong, and there is no energy consumption generated by two-fire billeting and environmental problems caused by heat treatment waste liquid. It can be shipped and used after it goes offline, which improves production efficiency.

[0031] The present invention adopts square billet one-fire material to produce 87SiMn ultra-high strength bridge cable steel, and the cost is 300-500 yuan / ton lower than that of two-fire material, and 800-1000 yuan / ton lower than that of salt bath / lead bath wire rod. The product competitiveness is strong, and there is no energy consumption generated by two-fire billet opening and environmental problems caused by heat treatment waste liquid. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is the metallographic structure photograph of the 87SiMn wire rod for high-strength bridge cables obtained in Example 1 (*500 times).

[0033] Figure 2 This is the metallographic structure photograph of the 87SiMn wire rod for high-strength bridge cables obtained in Example 2 (*500 times).

[0034] Figure 3 Photo of the wire rods entering the insulation corridor. DETAILED DESCRIPTION

[0035] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.

[0036] The wire rod for high-strength bridge cables of the present invention is wire rod 87SiMn, and the chemical composition and weight percentage of the wire rod 87SiMn are: C: 0.85-0.92%, Si: 1.2-1.5%, Mn: 0.90-1.0%, Cr: 0.30-0.35%, P≤0.015%, S≤0.010%, Ni≤0.10%, Cu≤0.10%, Al≤0.04%, [O]≤0.001%, [N]≤0.006%, Sn≤0.0100%, As≤0.0100%, and the rest are Fe and unavoidable impurities.

[0037] The production process of high-strength wire rod for bridge cables is: hot metal pretreatment → BOF (BOF refers to converter) → LF refining → VD vacuum furnace treatment → 180*180mm 2 Continuous casting → slow cooling of billet → high-speed wire rolling.

[0038] Special molten iron and clean scrap steel are used for steelmaking; constant pulling speed, low superheat pouring, strong cooling process, electromagnetic stirring of crystallizer, electromagnetic stirring at the end, light and heavy pressure reduction and full protection pouring are adopted for continuous casting; after the billet is slowly cooled, reasonable controlled rolling and controlled cooling process is adopted for rolling.

[0039] The chemical composition and weight percentage of the wire rod 87SiMn are:

[0040] C: 0.87%, Si: 1.35%, Mn: 0.95%, Cr: 0.32%, P: 0.006%, S: 0.003%, Ni: 0.02%, Cu: 0.03%, Al: 0.03%, O: 0.0008%, N: 0.005%, Sn: 0.0012%, As: 0.0043%, the balance is iron and inevitable impurities; or C: 0.88%, Si: 1.38%, Mn: 0.96%, Cr: 0.31%, P: 0.007%, S: 0.002%, Ni: 0.02%, Cu: 0.03%, Al: 0.03%, O: 0.0007%, N: 0.005%, Sn: 0.0013%, As: 0.0041%, the balance is iron and inevitable impurities.

[0041] The wire rod strength reaches above 1400MPa.

[0042] The wire rod meets the technical requirements for producing ultra-high strength bridge cables with a Φ single wire specification of 5.0 mm and a strength level of 2200-2300 MPa.

[0043] The production method of the high-strength wire rod for bridge cables of the present invention comprises the following steps:

[0044] (1) Converter smelting: In order to control harmful residual elements, special molten iron is selected, and the sulfur content of the molten iron is reduced through molten iron pretreatment.

[0045] The converter adopts the double slag method to effectively reduce the phosphorus content, and the slide plate is used to block the slag during steel discharge to prevent slag from falling from the converter, thereby controlling the purity of the molten steel from the source.

[0046] (2) LF refining: LF refining uses aluminum particles for diffusion deoxidation, the white slag time is kept above 20 minutes, and the slag system adopts a ternary slag system.

[0047] (3) VD vacuum treatment: Maintain high vacuum less than 67Pa for ≥12 minutes to reduce the gas content in molten steel.

[0048] (4) Continuous casting: Continuous casting uses 180*180mm 2 The production is carried out in sections, and the integral tundish is used for full protection casting. The continuous casting furnace pulling speed is controlled at 1.6m / min, the superheat is stabilized at 20-30℃, and the crystallizer, end electromagnetic stirring, light and heavy pressure reduction technology are used. The cooling method of water cooling and aerosol cooling in the continuous casting second cooling section is adopted to reduce the columnar crystal area, increase the equiaxed crystal area, prevent the development of columnar crystals, reduce the component segregation of molten steel during the solidification process, and improve the core and surface quality of the continuous casting billet. Specific parameters: crystallizer electromagnetic stirring current 400A, frequency 3.5Hz, end electromagnetic stirring current 700A, frequency 10Hz, continuous casting second cooling zone specific water volume 0.45L / Kg, total pressure reduction 25mm.

[0049] Slow cooling of steel billet: After slow cooling of steel billet for 24 hours, hot rolling is carried out;

[0050] (5) Rolling: A walking beam heating furnace is used, with a total of 30 rolling mills. The finishing rolling adopts the "8+4" mode, i.e., finishing rolling unit + sizing unit rolling, and the online diameter gauge is used to measure the wire rod size in real time to ensure that the wire rod size accuracy reaches Class C accuracy. The main process parameters of the rolling are: heating furnace heating stage 1000°C, heating stage 2 1160°C, equalizing stage 1180°C, finishing mill 870°C, sizing mill 900°C, wire laying 840°C~860°C; roller speed 0.7m / s; total heating time of the heating furnace 120~180min. The air cooling parameters of the Stelmor air cooling line are: a total of 14 fans are turned on, and the rated air volume of each fan is 200,000 m 3 / h, wind pressure 3000Pa.

[0051] The present invention adopts square billet one-fire material to produce 87SiMn ultra-high strength stranded wire steel, and the cost is 300-500 yuan / ton lower than that of two-fire material, and 800-1000 yuan / ton lower than that of salt bath / lead bath wire rod. The product has strong competitiveness, and there is no energy consumption generated by two-fire billet opening and environmental problems caused by heat treatment waste liquid.

[0052] Example 1

[0053] The production method of wire rod 87SiMn for high-strength bridge cables in this embodiment, the chemical composition and weight percentage of the wire rod 87SiMn are: C: 0.87%, Si: 1.35%, Mn: 0.95%, Cr: 0.32%, P: 0.006%, S: 0.003%, Ni: 0.02%, Cu: 0.03%, Al: 0.03%, O: 0.0008%, N: 0.005%, Sn: 0.0012%, As: 0.0043%, and the remainder is iron and unavoidable impurities.

[0054] This embodiment 1 ensures the mechanical properties of the steel wire rod for ultra-high strength stranded wire by reasonably matching the elements such as C, Si, Mn, Cr, Al in the composition, reduces the heat treatment process and the process of opening the large square billet, and saves production costs. Among them, the C content is 0.87%. The level of C content is the main factor determining the tensile strength of the wire rod, but too high C is prone to central segregation, which seriously affects the quality of the rolled material. Therefore, by reasonably matching the content of C, Si, and Cr elements, the wire rod has a high tensile strength. The Si content is 1.35%. Si can improve the hardenability and tensile strength of steel. At the same time, adding Si to the molten steel has a good deoxidation effect and can purify the molten steel. The Cr content is 0.35%. The Cr element can improve the tensile strength of the wire rod. If the content is too low, the strength of the wire rod will be insufficient. If the content is too high, the wire rod will produce abnormal structures such as martensite during the rolling and cooling process, which seriously affects the drawing of the steel wire. The Al content is 0.03%. Al can be added into the molten steel as a deoxidizer to purify the molten steel. At the same time, an appropriate amount of Al can play a role in refining the grains.

[0055] The production process of high-strength wire rod for bridge cables is: hot metal pretreatment → BOF (converter) → LF refining → VD vacuum furnace treatment → 180*180mm 2 Continuous casting → slow cooling of billet → high-speed wire rolling.

[0056] The production method of the high-strength wire rod for bridge cables of this embodiment comprises the following steps:

[0057] (1) Converter smelting: The converter adopts the double slag method, and the steel tapping uses a slide plate to block the slag;

[0058] (2) LF refining: LF refining uses aluminum particles for diffusion deoxidation, the white slag time is kept above 20 minutes, and the slag system adopts a ternary slag system;

[0059] (3) VD vacuum treatment: During the VD vacuum treatment, the vacuum degree is below 67Pa, the time is ≥12 minutes, the hydrogen content in the molten steel is controlled below 1.5ppm, and the superheat of the tundish is controlled at 20-30℃;

[0060] (4) Continuous casting: adopt full-process protection pouring, constant casting speed production, low superheat pouring, use of crystallizer, end electromagnetic stirring, light and heavy pressure reduction technology, and combined with the strong cooling process of water cooling + mist cooling in the secondary cooling zone;

[0061] (5) Rolling: The rolling process adopts a walking beam heating furnace, and the finishing rolling adopts the "8+4" mode, i.e., the finishing rolling unit + the sizing unit rolling. The wire rod size is measured in real time by an online diameter gauge, and the wire rod is cooled by a Stelmor air cooling line and insulated by an insulation corridor.

[0062] In the production process of manufacturing wire rods in this embodiment 1, the temperature of the molten steel after VD vacuum treatment is 1505°C, the superheat of the tundish is controlled at 25°C, the continuous casting speed is controlled at 1.6m / min, the crystallizer electromagnetic stirring current is 400A, the frequency is 3.5Hz, the end electromagnetic stirring current is 700A, the frequency is 10Hz, the specific water volume is 0.45L / Kg, and the total pressure reduction is 25mm.

[0063] Step (4) After the continuous casting, the steel billet is slowly cooled for 24 hours and then heated and rolled.

[0064] Rolling process parameters: heating furnace heating stage 1000℃, heating stage 2 1160℃, equalizing stage 1180℃, finishing mill 870℃, warp reduction 900℃, wire laying 850℃; roller speed 0.7m / s; total heating time of heating furnace 135min. Air cooling parameters: the first 6 fans are all running at full load, 7 to 14 fans are opened at 70%, the rated air volume of each fan is 200,000 m3 / h, and the wind pressure is 3000Pa. Rapid strong cooling is achieved through the Stelmor air cooling line, which suppresses abnormal structures such as martensite. The temperature entering the insulation corridor is 450-500℃, and the insulation time is 125 minutes. A sorbite structure with high strength and good plasticity is generated. The sorbite structure content reaches 95%, such as Figure 1 shown.

[0065] The tensile strength of the ultra-high strength wire rod 87SiMn produced in Example 1 is 1425MPa, the network carbide is evenly distributed, the network carbon level is ≤1.0, and no martensite appears. The actual strength of the finished single wire of the 5.0mm specification 2300Mpa grade steel wire made by the wire rod is 2250MPa.

[0066] Example 2

[0067] The parameters not described in this embodiment are the same as those in Embodiment 1.

[0068] The wire rod 87SiMn for high-strength bridge cables of this embodiment 2 is different from that of embodiment 1 in that the chemical composition and weight percentage of the wire rod 87SiMn are as follows: C: 0.88%, Si: 1.38%, Mn: 0.96%, Cr: 0.31%, P: 0.007%, S: 0.002%, Ni: 0.02%, Cu: 0.03%, Al: 0.03%, O: 0.0007%, N: 0.005%, Sn: 0.0013%, As: 0.0041%, and the rest

[0069] The content is iron and inevitable impurities.

[0070] In the production process of manufacturing wire rod in this embodiment 2, the temperature of molten steel after VD vacuum treatment is 1506℃, the superheat of the tundish is controlled at 25℃, the continuous casting speed is controlled at 1.6m / min, the electromagnetic stirring current of the crystallizer is 400A, and the frequency is 3.5Hz. The terminal electromagnetic stirring current is 700A, the frequency is 10Hz, the specific water volume is 0.45L / Kg, and the total reduction is 25mm. Rolling process parameters: heating furnace heating stage 1000℃, heating stage 2 1160℃, equalizing stage 1180℃, finishing mill temperature 870℃, warp reduction temperature 900℃, wire laying temperature 850℃; roller speed 0.7m / s; total heating time of the heating furnace 136min, air cooling parameters are: 14 fans, of which the 1st to 6th fans are running at full load, 7th to 14th fans are opened at 70%, and the rated air volume of each fan is 200,000m 3 / h, wind pressure 3000Pa. The temperature of the heat preservation corridor is 450~500℃, and the heat preservation time is 125 minutes. Under this process, the content of sorbite in the rolled wire rod reaches 96%. Figure 2 shown.

[0071] The tensile strength of the ultra-high strength wire rod 87SiMn produced in Example 2 is 1435MPa, the network carbide is evenly distributed, the network carbon level is ≤1.0, and no martensite appears. The actual strength of the finished single wire of the 5.0mm specification 2300Mpa grade steel wire made by the wire rod is 2260MPa.

[0072] Comparative Example 1

[0073] In this comparative example, except that the Si content in the chemical composition of the wire rod 87SiMn is 1.0%, other parameters and operations are the same as those of Example 1.

[0074] Comparative Example 2

[0075] In this comparative example, except that the Mn content in the chemical composition of the wire rod 87SiMn is 0.7%, other parameters and operations are the same as those of Example 1.

[0076] Comparative Example 3

[0077] In this comparative example, except that the Cr content in the chemical composition of the wire rod 87SiMn is 0.2%, other parameters and operations are the same as those of Example 1.

[0078] Comparative Example 4

[0079] In this comparative example, except that the number of fans of wire rod 87SiMn is 1 to 14, 100%, the other parameters and operations are the same as those of Example 1.

[0080] The performance test results of the wire rods and steel wires obtained in various embodiments and comparative examples are shown in Table 1.

[0081] Table 1 Performance test results of wire rods and steel wires obtained in various embodiments and comparative examples

[0082]

Claims

1. A high-strength wire rod for bridge cables, which is wire rod 87SiMn, It is characterized in that The chemical composition and weight percentage of the wire rod 87SiMn are: C: 0.85-0.92%, Si: 1.2-1.5%, Mn: 0.90-1.0%, Cr: 0.30-0.35%, P≤0.015%, S≤0.010%, Ni≤0.10%, Cu≤0.10%, Al≤0.04%, [O]≤0.001%, [N]≤0.006%, Sn≤0.0100%, As≤0.0100%, and the rest are Fe and unavoidable impurities.

2. The high-strength wire rod for bridge cables according to claim 1, It is characterized in that The strength of 87SiMn wire rod with a diameter of 14mm reaches over 1400MPa.

3. The high-strength wire rod for bridge cables according to claim 1 or 2, It is characterized in that The wire rod 87SiMn meets the technical requirements for producing ultra-high strength bridge cables with a single wire specification of Φ5.0mm and a strength level of 2200-2300MPa.

4. The method for producing a high-strength wire rod for bridge cables according to any one of claims 1 to 3, It is characterized in that The following steps are involved: (1) Converter smelting: The converter adopts the double slag method, and the steel tapping uses a slide plate to block the slag; (2) LF refining: LF refining uses aluminum particles for diffusion deoxidation, the white slag time is kept above 20 minutes, and the slag system adopts a ternary slag system; (3) VD vacuum treatment: During the VD vacuum treatment, the vacuum degree is below 67Pa, the time is ≥12 minutes, the hydrogen content in the molten steel is controlled below 1.5ppm, and the superheat of the tundish is controlled at 20-30℃; (4) Continuous casting: adopt full-process protection pouring, constant casting speed production, low superheat pouring, use of crystallizer, end electromagnetic stirring, light and heavy pressure reduction technology, and combined with the strong cooling process of water cooling + mist cooling in the secondary cooling zone; (5) Rolling: The rolling process adopts a walking beam heating furnace, and the finishing rolling adopts the "8+4" mode, i.e., the finishing rolling unit + the sizing unit rolling. The wire rod size is measured in real time by an online diameter gauge, and the wire rod is cooled by a Stelmor air cooling line and insulated by an insulation corridor.

5. The method for producing high-strength wire rod for bridge cables according to claim 4, It is characterized in that During the continuous casting process of step (4), 180*180mm 2 Cross-section billet production; crystallizer electromagnetic stirring current 380-420A, frequency 3.4-3.6Hz; terminal electromagnetic stirring current 680-720A, frequency 9-11Hz; specific water volume 0.4-0.5L / Kg, total reduction 20-30mm.

6. The method for producing high-strength wire rod for bridge cables according to claim 5, It is characterized in that During the continuous casting process of step (4), 180*180mm 2 Cross-section billet production; crystallizer electromagnetic stirring current 400A, frequency 3.5Hz; end electromagnetic stirring current 700A, frequency 10Hz; specific water volume 0.45L / Kg, total pressure reduction 25mm.

7. The method for producing high-strength wire rod for bridge cables according to claim 4 or 5, It is characterized in that During the continuous casting of step (4), the casting speed is kept constant and the casting speed of the continuous casting furnace is controlled at 1-3 m / min; and / or, during the continuous casting of step (4), the superheat is kept stable at 20-30°C; and / or, after the continuous casting of step (4), the steel billet is slowly cooled for 24 hours and then heated and rolled.

8. The method for producing high-strength wire rod for bridge cables according to claim 4 or 5, It is characterized in that In step (5), the main process parameters of the rolling are: heating furnace heating stage 980-1020°C, heating stage 2 1140-1160°C, soaking stage 1170-1200°C, finishing mill 860-880°C, warp reduction 880-920°C, spinning 840-860°C; roller speed 0.6-0.8 m / s; total heating time in the heating furnace 120-180 min.

9. The method for producing high-strength wire rod for bridge cables according to claim 4 or 5, It is characterized in that In step (5), the air cooling parameters of the Stelmore air cooling line are: 13-15 fans, and the air volume of each fan is 180,000-220,000 m 3 / h, wind pressure 2800-3200Pa.

10. The method for producing high-strength wire rod for bridge cables according to claim 4 or 5, It is characterized in that In step (5), the process parameters of the insulation corridor are as follows: the temperature entering the insulation corridor is 400-500°C, and the insulation time is more than 120 minutes.

Citation Information

Cited By

  • Hot-rolled V-containing high-strength wire rod for 1860 MPa bridge cable and manufacturing method of hot-rolled V-containing high-strength wire rod

    CN119144801A

  • Hot-rolled wire rod for 2100 MPa bridge cable and manufacturing method of hot-rolled wire rod

    CN119303991A

  • A 2100MPa grade hot-rolled wire rod for bridge cables and a manufacturing method thereof

    CN119303991B

  • High-pulling-speed production process of 200mm*200mm continuous casting billet of high-carbon hard wire steel

    CN119426548A

  • High-strength complex-phase hot-rolled wire rod for 2400 MPa bridge cable and manufacturing method of high-strength complex-phase hot-rolled wire rod

    CN119956073A