Heat treatment process for 0Cr25Al5 wire rod

By adopting heat treatment process in 0Cr25Al5 wire, the steps of heating, insulation and rapid cooling are solved, the problem of brittle breakage of wire after hot rolling is improved, the elongation and tensile strength of wire are improved, and the stability of the pulling process is ensured. and productivity.

CN118880018APending Publication Date: 2024-11-01SHANXI TAIGANG STAINLESS STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410976785.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

0Cr25Al5 wire is prone to brittle breaking and breaking after hot rolling, resulting in problems during the drawing process.

Method used

The heat treatment process is adopted, including raising the heat treatment furnace from room temperature to 810 to 850°C, then loading the 0Cr25Al5 wire and insulating it for 1 to 3 hours, then quickly cooling to 70 to 100°C, and processing using a resistance furnace or a gas furnace.

Benefits of technology

The high elongation and stable tensile strength of the wire are achieved, and brittle breakage and fracture are avoided. The process flow is simple, the cycle is short and the production efficiency is high.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880018A_ABST
    Figure CN118880018A_ABST
Patent Text Reader

Abstract

The invention provides a heat treatment method aiming at the current situation that the 0Cr25Al5 wire rod is subjected to drawing cracking, brittle failure and low elongation after being subjected to hot rolling and acid pickling and cannot meet the drawing processing requirements of downstream users on materials, so that the elongation of the materials is stably improved, and the problem of drawing breakage of the materials is completely eradicated. The method comprises the following steps: heating a 0Cr25Al5 wire rod to 810-850 DEG C through a heat treatment process for optimizing the heating rate, the heat preservation temperature and time and the cooling temperature, and preserving heat for 1-3 hours; and then the workpiece is quickly put into water to be cooled to be below 100 DEG C, so that the ductility of the workpiece is remarkably improved, and the problems of brittle fracture and fracture during drawing of the 0Cr25Al5 wire rod are fundamentally solved. The wire rod subjected to heat treatment by adopting the process method disclosed by the invention is uniform in tensile strength, relatively high in ductility and relatively good in plasticity, and the problems of drawing brittle failure and fracture of the 0Cr25Al5 wire rod after hot rolling are fundamentally solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloy material heat treatment, in particular to a 0Cr25Al5 wire material heat treatment process. Background Art

[0002] 0Cr25Al5 wire is a high-performance electric heating alloy, which is suitable for normal use in high temperature environments below 1250 degrees. This alloy has the characteristics of high resistivity, low specific gravity, excellent heat resistance, and good oxidation resistance. It has good corrosion resistance at high temperatures and is especially suitable for use in atmospheres containing sulfur, sulfides, and various hydrocarbon gases. It is also inexpensive and widely used in electric heating elements, precision instruments, chemical containers, and other industries. The disadvantage is that the hot-rolled wire rod has low high-temperature strength, poor plasticity, and is easy to break. The hot-rolled pickled wire rod often breaks after drawing.

[0003] The present invention aims to provide an efficient 0Cr25Al5 wire heat treatment process to solve the problem of brittle fracture and breakage of 0Cr25Al5 wire after hot rolling. Summary of the invention

[0004] The purpose of the present invention is to provide a 0Cr25Al5 wire heat treatment process in view of the above problems.

[0005] The object of the present invention is achieved as follows: 1. A 0Cr25Al5 wire heat treatment process, comprising the following steps: Step 1: hot charging process, heating the heat treatment furnace from room temperature to 810-850°C at a heating rate of 3-10°C / min; Step 2: loading the 0Cr25Al5 wire into the heat treatment furnace, heating the temperature in the furnace to 810-850°C at a heating rate of 3-10°C / min, and keeping it warm for 1-3 hours; Step 3: after the insulation is completed, placing the 0Cr25Al5 wire into water within 5-40s and cooling it to 70-100°C before taking it out of the furnace.

[0006] The heat treatment furnace is a resistance furnace or a gas furnace.

[0007] The beneficial effects of the present invention are as follows: the heat treatment process of the present invention adopts appropriate heating rate, holding time, cooling temperature and time, and has the advantages of uniform annealing performance, simple process flow, short heat treatment cycle and high production efficiency.

[0008] The wire treated by the process method of the present invention has a high elongation and is stable at 25% to 34%. Under the same process, the tensile strength fluctuates slightly, with a maximum of 15 MPa. There is no brittle fracture or breakage after pickling and drawing. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] The present invention will be further described below in conjunction with the accompanying drawings.

[0010] Figure 1 This is a heat treatment process diagram of Example 1 of the present invention.

[0011] Figure 2 This is a heat treatment process diagram of Example 2 of the present invention.

[0012] Figure 3 This is a heat treatment process diagram of Example 3 of the present invention. DETAILED DESCRIPTION

[0013] The technical scheme of the present invention is: adopt the hot charging furnace process, first heat the heat treatment furnace to 810-850℃, after the furnace temperature reaches the requirement, quickly load the wire rod into the heat treatment furnace, immediately set the furnace temperature to 830±20℃ after the wire rod enters the furnace, keep it warm for 1-3h, quickly take it out of the furnace and cool it in water after the insulation is over, and take it out of the water after the coil is completely immersed in water for 5-40s, and the surface temperature of the wire rod after it is wetted with water is 70-100℃. No nitrogen is passed throughout the process. The specific technical scheme is as follows: A 0Cr25Al5 wire heat treatment process comprises the following steps: step 1: adopting a hot charging process, heating a heat treatment furnace from room temperature to 810-850°C at a heating rate of 3-10°C / min; step 2: immediately loading the 0Cr25Al5 wire into the heat treatment furnace, heating the temperature in the furnace to 810-850°C at a heating rate of 3-10°C / min, and keeping the temperature for 1-3 hours; step 3: after the insulation is completed, putting the 0Cr25Al5 wire into water within 5-40 seconds, cooling it to 70-100°C, and then taking it out of the furnace; Preferably, the heat treatment furnace mentioned above is a resistance furnace or a gas furnace. Example 1

[0014] A 0Cr25Al5 wire heat treatment process comprises the following steps: step 1: adopting a hot charging process, heating a heat treatment furnace from room temperature to 810°C at a heating rate of 5-10°C / min; step 2: immediately loading the 0Cr25Al5 wire into the heat treatment furnace, heating the temperature in the furnace to 820°C at a heating rate of 5-10°C / min, and keeping the temperature for 3 hours; step 3: after the insulation is completed, placing the 0Cr25Al5 wire into water and cooling it to 70-80°C within 30s.

[0015] The wire treated in this example was subjected to a pulling test, and the tensile strength was uniform and the elongation was high, meeting the internal control requirements. Example 2

[0016] A 0Cr25Al5 wire heat treatment process comprises the following steps: step 1: adopting a hot charging process, heating a heat treatment furnace from room temperature to 820°C at a heating rate of 3-5°C / min; step 2: immediately loading the 0Cr25Al5 wire into the heat treatment furnace, heating the temperature in the furnace to 830°C at a heating rate of 3-5°C / min, and keeping the temperature for 2 hours; step 3: after the insulation is completed, placing the 0Cr25Al5 wire into water and cooling it to 80-90°C within 40s. Example 3

[0017] A 0Cr25Al5 wire heat treatment process comprises the following steps: step 1: adopting a hot charging process, heating a heat treatment furnace from room temperature to 840°C at a heating rate of 3-5°C / min; step 2: immediately loading the 0Cr25Al5 wire into the heat treatment furnace, heating the temperature in the furnace to 840°C at a heating rate of 3-5°C / min, and keeping the temperature for 1.5 hours; step 3: after the insulation is completed, placing the 0Cr25Al5 wire into water and cooling it to 90-100°C within 40s.

[0018] In Examples 1 to 3, the method of GB / T 228-1987 was used to perform metal tensile tests on the heat-treated workpieces. The test values ​​are shown in Table 1.

[0019]

[0020] The mechanical property results of Examples 1 to 3 show that the wire material treated by the process method of the present invention has the advantage of uniform heat treatment performance. At the same time, the treated wire material has high ductility and good plasticity, is suitable for subsequent drawing processing, and eliminates product cracking and brittle fracture.

[0021] The above description is only a specific embodiment of the present invention, but the structural features of the protection scope of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are all covered by the patent scope of the present invention.

Claims

1. A 0Cr25Al5 wire heat treatment process, characterized in that: The steps include: Step 1: hot charging process, heating the heat treatment furnace from room temperature to 810-850℃ at a heating rate of 3-10℃ / min; Step 2: Load the 0Cr25Al5 wire into the heat treatment furnace, and raise the temperature in the furnace to 810-850°C at a heating rate of 3-10°C / min, and keep it warm for 1-3 hours; Step 3: After the insulation is completed, put the 0Cr25Al5 wire into water and cool it to 70-100℃ within 5-40s before taking it out of the furnace.

2. A 0Cr25Al5 wire heat treatment process according to claim 1, characterized in that: The heat treatment furnace is a resistance furnace or a gas furnace.