Aluminum relieved tooth radiator profile, extrusion production method and application of aluminum relieved tooth radiator profile
By adopting smelting casting and extrusion processes in the production of aluminum shovel radiator profiles, combined with quenching and straightening treatment, the production stability and low product pass rate of high-toothed aluminum shovel radiator profiles are solved, and the problem of high-toothed aluminum shovel radiator profiles is achieved. More efficient production and lower costs.
Patent Information
- Application Number
- CN202410863465.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-29
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-06-29
AI Technical Summary
The existing aluminum shovel radiator profiles have poor production stability, serious coarse crystal problems, uneven grain size, unsatisfactory low-speed structure, bending teeth, broken teeth, uneven tooth surface, Defects such as tooth burrs lead to low product pass rate and high raw material loss.
The casting rod is prepared by melt casting method, controlling the composition and refining process of the casting ingot, combining extrusion and quenching treatment, controlling the extrusion speed, quenching cooling method and straightening elongation rate, ensuring the grain size and hardness of the profile, avoiding bending teeth, Defects such as broken teeth, and tissue structure is improved by spraying water cooling and casting deteriorating agents.
It effectively overcomes the coarse crystal, pinhole defects, and uneven hardness problems of aluminum shovel tooth radiator profiles, improves the qualification rate of finished products, reduces raw material loss and production cost, and improves production efficiency. It is suitable for high-toothed aluminum shovel tooth radiator Preparation.
Smart Images

Figure CN118880079A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of aluminum skived-tooth radiator profiles, and in particular to an aluminum skived-tooth radiator profile, an extrusion production method and applications thereof. Background Art
[0002] As a device for conducting and dissipating heat, radiators are widely used in new energy vehicles, photovoltaic energy storage inverters, wind power generation, electronic communications, 5G base stations, charging piles, smart devices, etc. Radiators are roughly divided into copper, cast iron, steel and aluminum alloy according to their materials. Among them, aluminum alloy radiators have the advantages of light weight, corrosion resistance, beautiful appearance, high cost performance and diversified shapes, and have been increasingly favored in recent years. Existing aluminum alloy radiators can be divided into extruded radiators, skived radiators, slotted radiators and other types according to different processing methods. Among them, skived radiators are known for their high thermal efficiency, light weight and small size. In recent years, the heat dissipation efficiency of skived radiators has been continuously improved, and they are widely used in many fields such as construction, automobiles, industry, aerospace, photovoltaic new energy, etc.
[0003] The existing skived-tooth radiator production process usually uses a skived-tooth machine to process the heat dissipation teeth on the extruded aluminum plate or hot-rolled aluminum plate, and then saws them to obtain the extruded aluminum plate skived-tooth radiator and the hot-rolled aluminum plate skived-tooth radiator respectively. Among them, the hot-rolled aluminum plate skived-tooth radiator has problems such as large aluminum material loss and high production cost, and currently has a trend of being replaced by the extruded aluminum plate skived-tooth radiator; at the same time, the extruded aluminum plate skived-tooth radiator can also solve the shortcomings of the traditional one-time extrusion molding process, such as the difficulty of extrusion discharge and the inability to achieve ultra-high-tooth extrusion, and can produce high-density, large-tooth-height, and high-tooth-number ultra-wide radiators, thereby obtaining better heat dissipation efficiency and air ducts, which are about 30% higher than the traditional aluminum alloy extruded radiator. In addition, because the cross-section of the extruded profile is relatively simple, the requirements for the extrusion die in the production process can be significantly reduced, and the product production efficiency can be further improved. As a result, in recent years, the research and development and application of high-tooth extruded aluminum plate skived-tooth radiators have become more and more.
[0004] Although the extruded aluminum plate skived-tooth radiator has all the above advantages, it has extremely high requirements on the extruded aluminum plate material and extrusion production process. The extruded aluminum plate profiles in the production process are prone to problems such as bent teeth, broken teeth, uneven tooth surface, and burrs on the tooth pieces. The qualified rate of finished products is low and the loss of raw materials is high. For example, the skived-tooth radiator profiles produced by extrusion using national standard aluminum bars as raw materials have obvious coarse grains on the profile surface and a large number of pinhole defects on the cross section. In addition, after skiving, there are defects such as bent teeth, broken teeth, uneven tooth surface, and burrs on the tooth pieces, which cannot be effectively overcome. At the same time, the production efficiency of the extrusion production of aluminum skived-tooth radiator profiles still needs to be further improved.
[0005] Furthermore, the inventors have discovered through research that the existing high-tooth (tooth height to tooth spacing ratio greater than 40) aluminum skived-tooth radiator profile extrusion production process has poor production stability, and the extruded aluminum plate profiles obtained by extrusion and air cooling have serious coarse grain problems, uneven grain size, and unsatisfactory low-magnification structure; and the skived teeth of the high-tooth aluminum skived-tooth radiator produced are more likely to be slightly bent, and the qualified rate of finished products is low. Summary of the invention
[0006] In order to solve the technical problems existing in the prior art, the present invention provides an aluminum skived-tooth radiator profile, an extrusion production method and its application, which is aimed at the poor production stability in the extrusion production process of aluminum skived-tooth radiator profile with high teeth (the ratio of tooth height to tooth spacing is greater than 40), the serious coarse crystal problem, uneven grain size and unsatisfactory low-magnification structure in the extruded aluminum plate profile obtained by extrusion and air cooling, and can avoid the problems of bent teeth or slightly bent teeth, broken teeth, uneven tooth surface, burrs on tooth pieces, uneven hardness and other undesirable problems in the extruded profile, improve the qualified rate of finished products, and reduce raw material loss; at the same time, further improve the production efficiency of the extrusion production of aluminum skived-tooth radiator profiles.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows: An extrusion production method for an aluminum skived-tooth radiator profile comprises the following steps: smelting, casting, and extrusion; The smelting and casting method comprises: melting and casting the ingot to obtain a cast rod with an average grain size of 135-137 μm; The ingot contains the following components in percentage: Si 0.1-0.13wt%, Mg≤0.03wt%, Fe≤0.15wt%, Cu≤0.03wt%, Mn≤0.03wt%, Cr≤0.03wt%, Zn≤0.03wt%, Ti≤0.03wt%, V≤0.03wt%, Al≥99.6wt%, and unavoidable impurities; The extrusion method comprises the following steps: controlling the extrusion speed to be 3-6 mm / s, extruding the cast rod, quenching the rod after extrusion, controlling the temperature of the profile entering the quenching zone to be 380-390° C., and the temperature of the profile exiting the quenching zone to be no greater than 40° C.; then controlling the stretching rate to be 1-2%, straightening the profile, and sawing the profile to obtain an aluminum skived-tooth radiator profile; The quenching cooling method is water spray cooling.
[0008] Preferably, during the extrusion, the extrusion die temperature is controlled to be 390-410°C, the extrusion barrel temperature is controlled to be 370-390°C, the casting rod temperature is controlled to be 350-370°C; and the extrusion pulling speed is controlled to be 2.6-3m / min.
[0009] Preferably, during the extrusion, the water spray flow rate of the water spray cooling is 0.65-0.75m 3 / h.
[0010] Furthermore, in the smelting and casting, the ingot is put into a melting and casting furnace, the melting and casting temperature is controlled to be 750-760°C, and the ingot is melted by stirring and keeping warm to obtain a melt; argon is introduced for the first refining and online degassing and slag removal; then a second refining and online degassing and slag removal are carried out, and after standing, a casting modifier is added at a temperature of 700-750°C, and the ingot is filtered and cast to obtain a cast rod.
[0011] Preferably, in the smelting and casting, the first refining temperature is 750-760°C, and the first refining time is 20-30min; The second refining temperature is 740-750℃, and the second refining time is 15-20min; The casting speed is 115-130 mm / min.
[0012] Preferably, in the smelting and casting, the casting modifier is aluminum titanium boron wire, and the amount of the casting modifier added to each ton of melt is 0.04-0.05wt%.
[0013] Preferably, in the smelting and casting, the ingot contains the following components in percentage: Si 0.12-0.13wt%, Mg 0.015-0.03wt%, Fe 0.1-0.15 wt%, Cu 0.015-0.03wt%, Mn 0.015-0.03wt%, Cr 0.015-0.03wt%, Zn 0.015-0.03wt%, Ti 0.015-0.03wt%, V 0.015-0.03wt%, Al≥99.6wt%, and inevitable impurities.
[0014] An aluminum skived-tooth radiator profile is produced by the production method as claimed in the preceding claim; the aluminum skived-tooth radiator profile has an average grain size of 66-90 μm, a Barcol hardness of 38-40 HBA, and a macrostructure coarse grain layer depth of ≤1 mm.
[0015] An application of the aforementioned aluminum skived-tooth radiator profile, the application of the aluminum skived-tooth radiator profile in the preparation of a high-multiple aluminum skived-tooth radiator; the high-multiple tooth multiple is not less than 43 times.
[0016] Furthermore, the toothing angle is controlled to be 11.7°, and the aluminum toothed radiator profile is subjected to toothing processing, the tooth spacing is controlled to be 1.5-1.6mm, the tooth thickness is 1.0-1.1mm, and the high-multiple tooth multiple is not less than 43 times; after the toothing processing is completed, the high-multiple tooth aluminum toothed radiator is obtained by milling the surface.
[0017] Compared with the prior art, the present invention has the following beneficial effects: 1. The extrusion production method of the aluminum skived-tooth radiator profile of the present invention adopts an improved composition ingot in the smelting and casting process, controls the Cu content to be 0.03wt% or less, reduces the Si and Fe contents, controls the Fe content to be slightly greater than the Si content, and appropriately controls the Cr, Ti, and V content; at the same time, in the smelting and casting process, sets a primary distillation and a secondary distillation, controls the hydrogen content of the melt to be ≤0.15mL / 100g, and controls the grain size of the profile; controls the specific extrusion speed, quenching cooling method, and straightening elongation in the extrusion process, and further controls the The grain size, hardness and coarse crystal layer depth of the profile can be adjusted to effectively overcome the serious coarse crystal defects, many pinhole defects, uneven grain size, uneven hardness, and unsatisfactory low-magnification structure of the aluminum skived-tooth radiator profile. The hardness and plasticity of the profile can be effectively adjusted to avoid defects such as bent teeth, broken teeth, uneven tooth surface, and burrs on the tooth pieces during the subsequent extrusion process of the profile. The bending rate of the skived teeth can be reduced to 0%, which can effectively improve the qualified rate of finished products, reduce raw material loss, and reduce production costs. At the same time, the production efficiency of the extrusion production of aluminum skived-tooth radiator profiles can be further improved.
[0018] 2. The extrusion production method of the aluminum skived-tooth radiator profile of the present invention can effectively overcome the problems of obvious coarse grains on the profile surface and many pinhole defects on the profile cross section in the production using national standard aluminum rod raw materials; the average grain size of the aluminum skived-tooth radiator profile obtained by extrusion is 66-90μm, the Bacol hardness is 38-40HBA, the macrostructure has no pinhole defects, the depth of the macrostructure coarse grain layer is less than 1mm, and the high-magnification microstructure has fine and uniform grains.
[0019] 3. The extrusion production method of the aluminum skived-tooth radiator profile of the present invention can efficiently extrude, quench and cool, and straighten the cast rod profile obtained by smelting and casting. There is no platform traffic jam during the processing, which effectively realizes the continuous production of the aluminum skived-tooth radiator profile, further improves production efficiency, reduces production costs, and is suitable for large-scale industrial production.
[0020] 4. The aluminum skived-tooth radiator profile of the present invention is used in the preparation of a high-multiple-tooth aluminum skived-tooth radiator. After skiving, a high-multiple-tooth aluminum skived-tooth radiator with a high-multiple tooth multiple of 43-50 times, a skived-tooth tooth spacing of 1.5-1.6 mm, a tooth thickness of 1.0-1.1 mm is obtained, a Bacol hardness of 38-40 HBA, and a skived-tooth tooth curvature of 0%. It can be effectively applied to working scenarios such as high-power inverters in photovoltaic energy storage stations that require the use of high-multiple-tooth aluminum skived-tooth radiators. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a 200-fold microstructure image of the aluminum skived-tooth radiator profile of Example 1; Figure 2This is a 500-fold microstructure image of the aluminum skived-tooth radiator profile of Example 1; Figure 3 This is a pinhole defect image of the aluminum profile cross section of Comparative Example 1; Figure 4 This is the "orange peel" defect image of the aluminum profile surface of Comparative Example 1; Figure 5 The diagram is a diagram showing the tooth bending of the skived-tooth radiator after the aluminum profile of Comparative Example 1 is skived; Figure 6 This is a picture of the unqualified finished product after the aluminum profile of comparative example 1 was processed with tooth skiving. DETAILED DESCRIPTION
[0022] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.
[0023] Example 1 This embodiment provides an extrusion production method for an aluminum skived-tooth radiator profile, and the specific steps are as follows: 1) Melting and casting The ingot includes the following components, by mass percentage: Si 0.12wt%, Mg 0.015wt%, Fe 0.1wt%, Cu0.015wt%, Mn0.015wt%, Cr 0.015wt%, Zn 0.015wt%, Ti 0.015wt%, V 0.015wt%, and the balance is Al (Al>99.6wt%), and inevitable impurities.
[0024] The ingot is melted and cast to obtain a cast rod with an average grain size of 135 μm.
[0025] Specifically, the ingot is put into a melting furnace, the melting temperature is controlled to 755°C, the ingot is kept warm and stirred for melting, and the melt is obtained; argon gas is introduced for the first refining and online degassing, the hydrogen content in the melt is controlled to be ≤0.15mL / 100g, the first refining temperature is 755°C, and after the first refining for 25 minutes, the slag is removed; then the second refining and online degassing are carried out, the second refining temperature is controlled to 745°C, and after the second refining for 17 minutes, the slag is removed; then it is allowed to stand for 20 minutes, and at a temperature of 720°C, a casting modifier is added, and after online double-stage filtration using 40-mesh and 60-mesh foam ceramic filter plates, casting is carried out, the casting speed is controlled to 120mm / min, and cast rods with an average grain size of 135μm are obtained.
[0026] Among them, the casting modifier is aluminum titanium boron wire, and the amount of casting modifier added to each ton of melt is 0.045wt%, that is, 0.45kg of aluminum titanium boron wire is added to each ton of melt.
[0027] 2) Squeeze The extrusion die temperature is controlled at 395°C, the extrusion barrel temperature is controlled at 380°C, the casting rod temperature is controlled at 360°C, the casting rod is extruded, the extrusion traction speed is controlled at 2.7m / min, and the extrusion speed is controlled at 3mm / s; after extrusion, quenching is performed, the temperature of the profile entering the quenching zone is controlled at 385°C, and the temperature of the profile exiting the quenching zone is controlled to be no more than 40°C; then the stretching rate is controlled to be 1%, the profile is straightened, and then sawed to obtain an extruded aluminum plate profile (i.e., aluminum skived tooth radiator profile); the average grain size of the aluminum skived tooth radiator profile is 66μm, the Babbitt hardness is 39HBA, the depth of the macrostructure coarse grain layer is 0.8mm, and the macrostructure has no pinhole defects. As shown in the attached manual Figure 1-2 As shown in the 200 times microstructure diagram and the 500 times microstructure diagram of the aluminum skived-tooth radiator profile obtained in this embodiment, it can be seen that the high-magnification microstructure grain size of the obtained aluminum skived-tooth radiator profile is uniform.
[0028] The quenching cooling method in the quenching zone is water spray cooling, and the water spray flow rate is 0.7m 3 / h.
[0029] This embodiment also provides an aluminum skived-tooth radiator profile produced by the extrusion production method of the aforementioned aluminum skived-tooth radiator profile.
[0030] The present embodiment also provides an application of the aluminum skived-tooth radiator profile in a high-multiple-tooth aluminum skived-tooth radiator. Specifically, the skived-tooth angle is controlled to be 11.7°, and the aluminum skived-tooth radiator profile is subjected to skived-tooth processing. The skived-tooth tooth spacing is controlled to be 1.5 mm, the tooth thickness is 1.0 mm, and the high-multiple tooth multiple is 50 times. After the skived-tooth processing is completed, the high-multiple-tooth aluminum skived-tooth radiator is obtained by milling the surface.
[0031] The high-tooth aluminum skived-tooth radiator has a Barcol hardness of 38 HBA and a tooth curvature of 0%.
[0032] Example 2 This embodiment provides an extrusion production method for an aluminum skived-tooth radiator profile, and the specific steps are as follows: 1) Melting and casting The ingot includes the following components, by mass percentage: Si 0.12wt%, Mg 0.015wt%, Fe 0.1wt%, Cu0.015wt%, Mn0.015wt%, Cr 0.015wt%, Zn 0.015wt%, Ti 0.015wt%, V 0.015wt%, and the balance is Al (Al>99.6wt%), and inevitable impurities.
[0033] The above ingot was used for melting and casting to obtain a cast rod with an average grain size of 136 μm.
[0034] Specifically, the ingot is put into a melting furnace, the melting temperature is controlled to 750°C, the ingot is kept warm and stirred for melting, and a melt is obtained; argon gas is introduced for the first refining and online degassing, the hydrogen content in the melt is controlled to be ≤0.15mL / 100g, the first refining temperature is 750°C, and after the first refining for 20 minutes, slag is removed; then a second refining and online degassing are carried out, the second refining temperature is controlled to 740°C, and after the second refining for 15 minutes, slag is removed; then it is allowed to stand for 15 minutes, and at a temperature of 700°C, a casting modifier is added, and after online double-stage filtration using 40-mesh and 60-mesh foam ceramic filter plates, casting is carried out, the casting speed is controlled to 115mm / min, and a cast rod with an average grain size of 136μm is obtained.
[0035] Among them, the casting modifier is aluminum titanium boron wire, and the amount of casting modifier added to each ton of melt is 0.04wt%, that is, 0.4kg of aluminum titanium boron wire is added to each ton of melt.
[0036] 2) Squeeze The extrusion die temperature is controlled at 390°C, the extrusion barrel temperature is controlled at 370°C, the cast rod temperature is controlled at 350°C, the cast rod is extruded, the extrusion traction speed is controlled at 2.6m / min, and the extrusion speed is controlled at 4mm / s; after extrusion, quenching is performed, the temperature of the profile entering the quenching zone is controlled at 380°C, and the temperature of the profile exiting the quenching zone is controlled to be no more than 40°C; then the stretching rate is controlled to be 1.2%, the profile is straightened, and then sawed to obtain an extruded aluminum plate profile (i.e., an aluminum skived-tooth radiator profile); the aluminum skived-tooth radiator profile has an average grain size of 72μm, a Babbitt hardness of 38HBA, a macrostructure coarse grain layer depth of 0.8mm, and a macrostructure without pinhole defects.
[0037] The quenching cooling method in the quenching zone is water spray cooling, and the water spray flow rate is 0.65m 3 / h.
[0038] This embodiment also provides an aluminum skived-tooth radiator profile produced by the extrusion production method of the aforementioned aluminum skived-tooth radiator profile.
[0039] The present embodiment also provides an application of the aluminum skived-tooth radiator profile in a high-multiple-tooth aluminum skived-tooth radiator. Specifically, the skived-tooth angle is controlled to be 11.7°, and the aluminum skived-tooth radiator profile is subjected to skived-tooth processing. The skived-tooth tooth spacing is controlled to be 1.55mm, the tooth thickness is 1.05mm, and the high-multiple-tooth multiple is 45 times. After the skived-tooth processing is completed, the high-multiple-tooth aluminum skived-tooth radiator is obtained by milling the surface.
[0040] The high-tooth aluminum skived-tooth radiator has a Barcol hardness of 38 HBA and a tooth curvature of 0%.
[0041] Example 3 This embodiment provides an extrusion production method for an aluminum skived-tooth radiator profile, and the specific steps are as follows: 1) Melting and casting The ingot includes the following components, by mass percentage: Si 0.12wt%, Mg 0.015wt%, Fe 0.1wt%, Cu0.015wt%, Mn0.015wt%, Cr 0.015wt%, Zn 0.015wt%, Ti 0.015wt%, V 0.015wt%, and the balance is Al (Al>99.6wt%), and inevitable impurities.
[0042] The above ingot was used for melting and casting to obtain a cast rod with an average grain size of 137 μm.
[0043] Specifically, the ingot is put into a melting furnace, the melting temperature is controlled to 760°C, the ingot is kept warm and stirred for melting, and the melt is obtained; argon gas is introduced for the first refining and online degassing, the hydrogen content in the melt is controlled to be ≤0.15mL / 100g, the first refining temperature is 760°C, and after the first refining for 30 minutes, the slag is removed; then the second refining and online degassing are carried out, the second refining temperature is controlled to 750°C, and after the second refining for 20 minutes, the slag is removed; then it is allowed to stand for 25 minutes, and at a temperature of 750°C, a casting modifier is added, and after online double-stage filtration using 40-mesh and 60-mesh foam ceramic filter plates, casting is carried out, the casting speed is controlled to 130mm / min, and cast rods with an average grain size of 137μm are obtained.
[0044] Among them, the casting modifier is aluminum titanium boron wire, and the amount of casting modifier added to each ton of melt is 0.05wt%, that is, 0.5kg of aluminum titanium boron wire is added to each ton of melt.
[0045] 2) Squeeze The extrusion die temperature is controlled at 410°C, the extrusion barrel temperature is controlled at 390°C, the cast rod temperature is controlled at 370°C, the cast rod is extruded, the extrusion traction speed is controlled at 2.8m / min, and the extrusion speed is controlled at 6mm / s; after extrusion, quenching is performed, the temperature of the profile entering the quenching zone is controlled at 390°C, and the temperature of the profile exiting the quenching zone is controlled to be no more than 40°C; then the stretching rate is controlled to be 2%, the profile is straightened, and then sawed to obtain an extruded aluminum plate profile (i.e., an aluminum skived-tooth radiator profile); the aluminum skived-tooth radiator profile has an average grain size of 90μm, a Babbitt hardness of 40HBA, a macrostructure coarse grain layer depth of 0.9mm, and a macrostructure without pinhole defects.
[0046] The quenching cooling method in the quenching zone is water spray cooling, and the water spray flow rate is 0.75m 3 / h.
[0047] The present invention also provides an aluminum skived-tooth radiator profile produced by the extrusion production method of the above-mentioned aluminum skived-tooth radiator profile.
[0048] The present invention also provides an application of the aluminum skived-tooth radiator profile in a high-multiple-tooth aluminum skived-tooth radiator. Specifically, the skived-tooth angle is controlled to be 11.7°, and the aluminum skived-tooth radiator profile is subjected to skived-tooth processing. The skived-tooth tooth spacing is controlled to be 1.6 mm, the tooth thickness is 1.1 mm, and the high-multiple tooth multiple is 43 times. After the skived-tooth processing is completed, the high-multiple-tooth aluminum skived-tooth radiator is obtained by milling the surface.
[0049] The high-tooth aluminum skived-tooth radiator has a Barcol hardness of 40 HBA and a tooth curvature of 0%.
[0050] Example 4 This embodiment provides an extrusion production method for an aluminum skived-tooth radiator profile, and the specific steps are as follows: 1) Melting and casting The ingot includes the following components, by mass percentage: Si 0.12wt%, Mg 0.015wt%, Fe 0.1wt%, Cu0.015wt%, Mn0.015wt%, Cr 0.015wt%, Zn 0.015wt%, Ti 0.015wt%, V 0.015wt%, and the balance is Al (Al>99.6wt%), and inevitable impurities.
[0051] The above ingot is used for melting and casting to obtain a cast rod with an average grain size of 125 μm.
[0052] Specifically, the ingot is put into a melting furnace, the melting temperature is controlled to be 755°C, the ingot is kept warm and stirred for melting, and the melt is obtained; argon gas is introduced for the first refining and online degassing, the hydrogen content in the melt is controlled to be ≤0.15mL / 100g, the first refining temperature is 755°C, and after the first refining for 25 minutes, the slag is removed; then the second refining and online degassing are carried out, the second refining temperature is controlled to be 745°C, and after the second refining for 17 minutes, the slag is removed; then it is allowed to stand for 20 minutes, and at a temperature of 720°C, a casting modifier is added, and after online double-stage filtration using 40-mesh and 60-mesh foam ceramic filter plates, casting is carried out, the casting speed is controlled to be 120mm / min, and cast rods with an average grain size of 125μm are obtained.
[0053] Among them, the amount of casting modifier added to each ton of melt is 0.05wt%, that is, 0.5kg of casting modifier is added to each ton of melt.
[0054] The casting modifier is a mixture of aluminum titanium boron wire and a modifier, and the weight ratio of the aluminum titanium boron wire to the modifier is 4:1.
[0055] The deterioration aid is prepared by the following method: The ammonium bifluoride solution, the mixed rare earth solution and the hexadecyltrimethylammonium bromide are mixed uniformly, and the temperature is increased to 65°C at a heating rate of 0.5°C / min, and the mixture is stirred at 150rpm for 220h, and then the mixture is transferred into a high-pressure reactor. After the high-pressure reactor is sealed, the temperature of the high-pressure reactor is controlled to be increased to 120°C, and the mixture is kept warm for 36h, and then the mixture is naturally cooled to room temperature. After the solid is separated, the solid is washed with deionized water to be neutral, and then dried at 90°C to constant weight in a vacuum environment of 0.08MPa to obtain nano rare earth fluoride. The nano rare earth fluoride and nano titanium dioxide are mixed uniformly at a weight ratio of 1:5 to obtain a deterioration aid.
[0056] Wherein, the ammonium bifluoride solution is an ammonium bifluoride aqueous solution with a concentration of 20wt%.
[0057] The mixed rare earth solution is an aqueous solution containing lanthanum nitrate, praseodymium nitrate and yttrium nitrate; the concentration of lanthanum nitrate is 8wt%, the concentration of praseodymium nitrate is 4wt%, and the concentration of yttrium nitrate is 2wt%.
[0058] The molar ratio of ammonium bifluoride, lanthanum nitrate, praseodymium nitrate, yttrium nitrate and hexadecyltrimethylammonium bromide is 10:0.8:0.4:0.2:1.
[0059] 2) Squeeze The extrusion die temperature is controlled at 395°C, the extrusion barrel temperature is controlled at 380°C, the cast rod temperature is controlled at 360°C, the cast rod is extruded, the extrusion traction speed is controlled at 2.7m / min, and the extrusion speed is controlled at 3mm / s; after extrusion, quenching is performed, the temperature of the profile entering the quenching zone is controlled at 385°C, and the temperature of the profile exiting the quenching zone is controlled to be no more than 40°C; then the stretching rate is controlled to be 1%, the profile is straightened, and then sawed to obtain an extruded aluminum plate profile (i.e., an aluminum skived-tooth radiator profile); the aluminum skived-tooth radiator profile has an average grain size of 61μm, a Babbitt hardness of 40HBA, a macrostructure coarse-grained layer depth of 0.6mm, a macrostructure without pinhole defects, and a macrostructure with uniform grain size.
[0060] The quenching cooling method in the quenching zone is water spray cooling, and the water spray flow rate is 0.7m 3 / h.
[0061] This embodiment also provides an aluminum skived-tooth radiator profile produced by the extrusion production method of the aforementioned aluminum skived-tooth radiator profile.
[0062] The present embodiment also provides an application of the aluminum skived-tooth radiator profile in a high-multiple-tooth aluminum skived-tooth radiator. Specifically, the skived-tooth angle is controlled to be 11.7°, and the aluminum skived-tooth radiator profile is subjected to skived-tooth processing. The skived-tooth tooth spacing is controlled to be 1.5 mm, the tooth thickness is 1.0 mm, and the high-multiple tooth multiple is 55 times. After the skived-tooth processing is completed, the high-multiple-tooth aluminum skived-tooth radiator is obtained by milling the surface.
[0063] The high-tooth aluminum skived-tooth radiator has a Barcol hardness of 40 HBA and a tooth curvature of 0%.
[0064] In this embodiment, an improved composition ingot is used in smelting and casting, the Cu content is controlled at 0.03wt% or less, the Si and Fe contents are reduced, and the Fe content is controlled to be slightly greater than the Si content, as well as appropriate Cr, Ti, and V; at the same time, in smelting and casting, primary distillation and secondary distillation are set, and the hydrogen content of the melt is controlled to be ≤0.15mL / 100g, and the grain size of the profile is controlled; after the refining is completed, aluminum titanium boron wire and a modification aid containing nano-fluoride rare earth and nano-titanium dioxide are used as a casting modification agent to further control the grain size of the profile, improve the stability of the profile in the subsequent processing process, and further improve the corrosion resistance of the profile, so as to obtain a cast rod with an average grain size of 125μm; then, a specific extrusion speed, quenching cooling method and straightening elongation are controlled in extrusion, The grain size, hardness and coarse crystal layer depth of the profile are further controlled, and the serious coarse crystal defects, many pinhole defects, uneven grain size, uneven hardness, and unsatisfactory low-magnification structure of the aluminum skived-tooth radiator profile are effectively overcome. The aluminum skived-tooth radiator profile with an average grain size of 61μm, a Bacol hardness of 40HBA, a low-magnification coarse crystal layer depth of 0.6mm, no pinhole defects in the low-magnification structure, and uniform grain size in the high-magnification structure is obtained; thereby effectively avoiding defects such as bent teeth, broken teeth, uneven tooth surfaces, and burrs on the tooth pieces during the subsequent extrusion process of the profile. In the preparation of aluminum skived-tooth radiators with a high-magnification tooth multiple of 55 times using the profile, the bending rate of the skived teeth is maintained at 0%, which effectively improves the qualified rate of finished products, reduces raw material loss, and reduces production costs; at the same time, the production efficiency of the extrusion production of aluminum skived-tooth radiator profiles is further improved.
[0065] Comparative Example 1 The technical solution of Example 1 is adopted, but the difference is that 1) the national standard 1060 aluminum rod is used for extrusion production, and the specific composition and percentage content of the aluminum rod are Si≤0.25wt%, Mg≤0.03wt%, Fe≤0.35 wt%, Cu≤0.05wt%, Mn≤0.03wt%, Zn≤0.05wt%, Ti≤0.03wt%, Al≥99.6wt%, and unavoidable impurities; 2) in the extrusion step, the extrusion speed is controlled to be 6mm / s, and the elongation is 2%; the cooling method is replaced by air cooling, and the air flow rate of the air cooling is 3m 3 / min.
[0066] The longest grain size of the profile obtained after extrusion treatment in Comparative Example 1 is 370 μm, the Barcol hardness is 48 HBA, the depth of the macrostructure coarse grain layer is 5 mm, the macrostructure surface coarse grain is obvious, and there are a large number of pinhole defects on the cross section (as shown in the attached manual). Figure 3 As shown in the figure), the profile surface has an "orange peel" defect (as shown in the attached manual Figure 4 At the same time, in the subsequent tooth-relief processing, the tooth curvature after tooth-relief exceeds 10% (as shown in the attached manual). Figure 5 and are prone to serious defects such as uneven tooth surface, broken teeth, and burrs on the teeth (see the attached manual). Figure 6 As shown), the qualified rate of finished products is low.
[0067] Furthermore, the temperature of the profile after extrusion is 385°C, and it requires about 2 hours of air cooling time before subsequent straightening treatment can be carried out, which can easily lead to traffic jams on the extrusion platform, inability to produce continuously, and low production efficiency.
[0068] Unless otherwise specified, all percentages used in the present invention are by mass.
[0069] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An extrusion production method for an aluminum skived-tooth radiator profile, characterized in that: It consists of the following steps: melting, casting and extrusion; The smelting and casting method comprises: melting and casting the ingot to obtain a cast rod with an average grain size of 135-137 μm; The ingot contains the following components in percentage: Si 0.1-0.13wt%, Mg≤0.03wt%, Fe≤0.15wt%, Cu≤0.03wt%, Mn≤0.03wt%, Cr≤0.03wt%, Zn≤0.03wt%, Ti≤0.03wt%, V≤0.03wt%, Al≥99.6wt%, and unavoidable impurities; The extrusion method comprises the following steps: controlling the extrusion speed to be 3-6 mm / s, extruding the cast rod, quenching the rod after extrusion, controlling the temperature of the profile entering the quenching zone to be 380-390° C., and the temperature of the profile exiting the quenching zone to be no greater than 40° C.; then controlling the stretching rate to be 1-2%, straightening the profile, and sawing the profile to obtain an aluminum skived-tooth radiator profile; The quenching cooling method is water spray cooling.
2. The extrusion production method of the aluminum skived-tooth radiator profile according to claim 1 is characterized in that: During the extrusion, the extrusion die temperature is controlled to be 390-410° C., the extrusion barrel temperature is controlled to be 370-390° C., the casting rod temperature is controlled to be 350-370° C.; and the extrusion pulling speed is controlled to be 2.6-3 m / min.
3. The extrusion production method of the aluminum skived-tooth radiator profile according to claim 1 is characterized in that: During the extrusion, the water spray flow rate of the water spray cooling is 0.65-0.75m 3 / h.
4. The extrusion production method of the aluminum skived-tooth radiator profile according to claim 1 is characterized in that: The smelting and casting process includes placing the ingot into a melting and casting furnace, controlling the melting and casting temperature to be 750-760°C, maintaining the temperature and stirring the ingot for melting, and obtaining a melt; introducing argon gas for the first refining and online degassing, and slagging; Then, the second refining is carried out and the steel is degassed online. After standing, a casting modifier is added at a temperature of 700-750°C, filtered, and cast to obtain cast rods.
5. The extrusion production method of the aluminum skived-tooth radiator profile according to claim 4 is characterized in that: In the smelting and casting, the first refining temperature is 750-760° C., and the first refining time is 20-30 min; The second refining temperature is 740-750℃, and the second refining time is 15-20min; The casting speed is 115-130 mm / min.
6. The extrusion production method of the aluminum skived-tooth radiator profile according to claim 4 is characterized in that: In the smelting and casting, the casting modifier is aluminum titanium boron wire, and the addition amount of the casting modifier in each ton of melt is 0.04-0.05wt%.
7. The extrusion production method of aluminum skived-tooth radiator profile according to claim 1, characterized in that: In the smelting and casting, the ingot contains the following components in percentage: Si 0.12-0.13wt%, Mg 0.015-0.03wt%, Fe 0.1-0.15 wt%, Cu 0.015-0.03wt%, Mn 0.015-0.03wt%, Cr 0.015-0.03wt%, Zn 0.015-0.03wt%, Ti 0.015-0.03wt%, V 0.015-0.03wt%, Al≥99.6wt%, and inevitable impurities.
8. An aluminum skived-tooth radiator profile, characterized in that: The aluminum skived-tooth radiator profile is produced by the production method according to any one of claims 1 to 7; the average grain size of the aluminum skived-tooth radiator profile is 66-90 μm, the Barcol hardness is 38-40 HBA, and the depth of the macrostructure coarse grain layer is ≤1 mm.
9. An application of the aluminum skived-tooth radiator profile according to claim 8, characterized in that: The aluminum skived-tooth radiator profile is used in the preparation of a high-multiple aluminum skived-tooth radiator; the high-multiple tooth multiple is not less than 43 times.
10. The use of the aluminum skived-tooth radiator profile according to claim 9, characterized in that: The toothing angle is controlled to be 11.7°, and the aluminum toothed radiator profile is subjected to toothing processing. The tooth spacing is controlled to be 1.5-1.6mm, the tooth thickness is 1.0-1.1mm, and the high-multiple tooth multiple is not less than 43 times. After the toothing processing is completed, the high-multiple tooth aluminum toothed radiator is obtained by milling the surface.
Citation Information
Patent Citations
Production method of powder-sprayed aluminium alloy sections
CN108220948A
Preparation method of aluminum profile for high-efficiency form relieved tooth
CN112680638A
Aluminum profile for relieved tooth radiator and extrusion production method of aluminum profile
CN115948681A
High-strength aluminum alloy extruded material with excellent corrosion resistance and method of producing the same
US20060243359A1
Method of manufacturing aluminum-containing composition and product made from such composition
US20130146188A1