Copper-iron alloy wire and preparation method and application thereof

By adopting copper-ferroalloy wire and three-stage smelting process, combining hot rolling solid solution and low-temperature aging annealing process, the problems of short service life and poor high-temperature resistance are solved, and high-temperature softening temperature and high-temperature corrosion resistance are achieved. The significant improvements extend the service life of the electrolytic iron core.

CN118880099APending Publication Date: 2024-11-01JINTIAN COPPER GROUP CORP NINGBO
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410861425.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing electrolyte has a short service life, poor resistance to high temperature softening, poor resistance to high temperature erosion, easy wear, affect welding quality and production efficiency, and high material cost.

Method used

Copper and ferroalloy wire material is used, containing Fe20%-50%, Cu margin, Ni 0.5%-1.0%, Cr 0.1%-0.5%, and combined process of hot rolling solid solution + aisle drawing + low-temperature aging annealing , and the copper-ferroalloy wire material with a high-temperature softening temperature above 600℃ and improved high-temperature corrosion resistance were prepared.

Benefits of technology

It significantly improves the high-temperature softening temperature and resistance to high-temperature corrosion of copper and ferroalloy wires, reduces the friction coefficient, extends the service life of the electrolyte iron core, and is suitable for high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880099A_ABST
    Figure CN118880099A_ABST
Patent Text Reader

Abstract

The invention discloses a copper-iron alloy wire as well as a preparation method and application thereof. The copper-iron alloy comprises the following components in percentage by mass: 20-50% of Fe, 0.5-1.0% of Ni, 0.1-0.5% of Cr and the balance of Cu. The copper-iron alloy comprises a matrix Cu phase, a Fe phase, a Cr phase, a Fe-Cr phase and a trace Cr3Ni2 phase. Wherein the particle size of Cr particles is 5-20 microns, the ratio of the particle size of Cr to the particle size of Fe is smaller than 1, and the ratio of Fe phase to Cr phase is larger than 200. According to the copper-iron alloy wire, the high-temperature softening temperature is 600 DEG C or above, the high-temperature corrosion resistance is high, the permeability reaches 0.01 mm or below at the temperature of 750 DEG C for 60 min, the friction coefficient is 0.2 or below (for steel), and the copper-iron alloy wire is more suitable for preparing the electric iron core.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper-iron alloy preparation, and in particular to a copper-iron alloy wire and a preparation method and application thereof. Background Art

[0002] Copper-iron alloy is a copper-iron alloy prepared by adding metallic iron to red copper. Because it has the electrical conductivity, thermal conductivity, ductility, elasticity, corrosion resistance, etc. of copper, and the wear resistance, hardness, magnetism, etc. of iron, as well as its unique high electromagnetic wave shielding, it is called electromagnetic compatible copper-iron alloy new material by the industry. As a new generation of high-end new materials of copper alloy, according to its performance, it can be applied to high-demand electromagnetic shielding boxes (boards), connectors, lead frames, electronic devices, motor coils and other products, and can also meet high-end needs such as electronic information, aerospace, transportation, etc. Therefore, this alloy system has a wide range of application fields and prospects for replacing old products, and has huge market potential. With the maturity of the industrialization of electronic appliances, its demand will surge, and the potential market is very large. At present, many domestic and foreign companies are committed to the research and development of iron-copper alloys, such as CFA in South Korea.

[0003] At present, copper is used in the processing of electric iron, but pure copper has several shortcomings in the application process: 1) poor resistance to high temperature softening, the high temperature softening temperature is only 350℃; 2) poor resistance to high temperature erosion, 750℃, 60min, penetration reaches 0.2mm, 3) easy to wear (for steel), the friction coefficient is 0.5, so the life is relatively short, need to be replaced frequently, affecting welding quality and production efficiency. In view of the above problems, it is urgent to develop a new alloy that is resistant to high temperature softening, corrosion and wear. Summary of the invention

[0004] The purpose of the present invention is to provide a copper-iron alloy wire and a preparation method and application thereof to address the problems in the prior art that electric iron has a short service life, affects the quality of welding products, and has high material costs.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] The first aspect is to provide a copper-iron alloy wire material, comprising the following components in mass percentage: Fe 20%-50%, and Cu as the balance.

[0007] Furthermore, the copper-iron alloy also includes Ni 0.5%-1.0% and Cr 0.1%-0.5%.

[0008] Furthermore, the copper-iron alloy includes a matrix Cu phase, a Fe phase, a Cr phase, a Fe-Cr phase and a trace amount of Cr3Ni2 phase; wherein the Cr particle size is 5-20 μm, the Cr particle size / Fe particle size is less than 1, and the Fe phase / Cr phase is greater than 200. A trace amount of single Cr phase is dispersed in the matrix and grain boundaries to inhibit the growth of grains, and at the same time, Fe-Cr intermetallic compounds are formed to inhibit the aggregation of iron phases.

[0009] The second aspect is to provide a method for preparing the copper-iron alloy wire, comprising the following steps:

[0010] Melting - horizontal continuous casting - hot rolling - wire drawing, straightening - aging annealing;

[0011] Among them, smelting: adopts multi-gradient graded insulation treatment.

[0012] Furthermore, the multi-gradient graded thermal insulation treatment has three or more gradients.

[0013] Furthermore, the multi-gradient graded insulation treatment specifically adopts a three-stage melting and insulation process: the raw materials are added to the smelting furnace, and after melting, the temperature is kept at 1150-1200°C for 1-3h, and then the temperature is increased to 1350°C-1400°C for 1-3h. After the insulation is completed, finally 1520°C-1580°C is used for insulation for 1-2h. After three stages of insulation, copper-chromium intermediate alloy is added, the crystallizer is assembled, the electromagnetic stirring device is put on, and traction begins.

[0014] Furthermore, the specific process of adding the raw materials is: adding electrolytic nickel and electrolytic copper plates into the continuous casting furnace, and after melting, setting the temperature at 1250°C-1300°C and then adding pure iron blocks.

[0015] Furthermore, in the process of adding pure iron blocks, it is necessary to use one or more of charcoal, graphite phosphorus sheets, and soot for covering, with a covering thickness of more than 100 mm, and activated carbon needs to be added at the same time; after three stages of insulation, the temperature is adjusted to 1400-1450°C, and then the copper-chromium intermediate alloy is added.

[0016] In the present invention, a three-stage smelting process is set up. The first stage is mainly above the melting point and above the peritectic line, and more saturated solid solutions and intermetallic compounds can be obtained to disperse copper and iron; the second stage is in the stage of sufficient mixing of liquid copper and iron, and mutual dissolution is promoted through the consistency of the face-centered crystal structure. Since the mutual reaction of copper and iron requires a long time, an intermediate stage is set; the third stage is mainly used to consolidate and improve the degree of mutual dissolution and the effect of sufficient mixing.

[0017] Furthermore, the specific parameters in the horizontal continuous casting process are set as: temperature 1350°C-1400°C, cooling water inlet and outlet temperature difference 60-80°C, and electromagnetic stirring frequency 20HZ-50HZ.

[0018] Furthermore, the pulling speed in the horizontal continuous casting process is 100-250 mm / min.

[0019] Further, the horizontal continuous casting process uses a strong cooling crystallizer, which includes a graphite sleeve, an electromagnetic stirring area, a primary cooling area and a secondary cooling area;

[0020] The graphite sleeve passes through the electromagnetic stirring area and the primary cooling area in sequence, and the outlet of the graphite sleeve faces the secondary cooling area;

[0021] The electromagnetic stirring region comprises: a thermal insulation layer and an electromagnetic stirrer, wherein the thermal insulation layer is arranged outside the graphite sleeve, and the electromagnetic stirrer is arranged outside the thermal insulation layer;

[0022] The primary cooling area adopts laminar cooling method;

[0023] The secondary cooling area adopts a cooling method with three gradients.

[0024] Furthermore, the primary cooling area includes: a copper sleeve, an iron sleeve, a laminar cooling zone, a water inlet and a water outlet, the copper sleeve is arranged on the outside of the graphite sleeve, the laminar cooling zone is arranged between the copper sleeve and the iron sleeve, and the water inlet and the water outlet are connected to the laminar cooling zone;

[0025] The secondary cooling area includes: a first water chamber, a second water chamber, a third water chamber, a cooling water distribution pipe, and a second cooling water chamber. The first water chamber, the second water chamber, and the third water chamber are sequentially arranged on the outside of the passage area of ​​the copper rod to be cooled. The first water chamber, the second water chamber, and the third water chamber respectively have water rings, and the copper rod to be cooled passes through three water rings in sequence. At the same time, the first water chamber, the second water chamber, and the third water chamber are respectively connected to the second cooling water chamber through the cooling water distribution pipe.

[0026] Furthermore, the hot rolling process is as follows: the continuous cast copper and iron bars are put into a trolley furnace, heated to 950-980°C, and kept warm for 30-60 minutes. After the heating is completed, the continuous cast copper and iron bars are rolled into Through hot rolling, the influence of iron particles on the grain boundaries of the structure can be eliminated at high temperature, while increasing the deformation plasticity of the material, thereby meeting the deformation requirements of copper and iron materials.

[0027] Furthermore, the aging annealing process is as follows: the straightened copper and iron wire is annealed in a trolley furnace at a temperature of 400°C-550°C and an annealing time of 2-4 hours. The combined process of hot rolling solid solution + wire drawing to increase distortion energy + low-temperature aging annealing at the end is adopted to make the material structure fine grains and the second phase fully precipitated, which ultimately reflects a significant increase in the strength and hardness of the material, greatly improved wear resistance, and an increase in the upper limit of application in high-temperature environments.

[0028] The third aspect is to provide the application of the above copper-iron alloy wire in the preparation of electric iron core.

[0029] The present invention adopts the above technical solution, and has the following technical effects compared with the prior art:

[0030] The present invention sets up a three-stage smelting process. The first stage is mainly above the melting point and above the peritectic line, and more saturated solid solutions and intermetallic compounds can be obtained to disperse copper and iron; the second stage is a stage in which liquid copper and iron are fully mixed, and mutual dissolution is promoted through the consistency of the face-centered crystal structure. Since the mutual reaction of copper and iron takes a long time, an intermediate stage is set; the third stage is mainly used to consolidate and improve the degree of mutual dissolution and the effect of full mixing.

[0031] The invention can quickly obtain highly saturated and uniformly mixed copper-iron materials by designing a strong cooling crystallizer, thereby ensuring that the copper-iron materials do not have a significant stratification problem.

[0032] The present invention adopts a combined process of hot rolling solid solution + channel drawing to increase distortion energy + low-temperature aging annealing at the end, so that the material structure has fine grains and the second phase is fully precipitated, which ultimately reflects a significant increase in the strength and hardness of the material, greatly improved wear resistance, and an increase in the upper limit of application in high-temperature environments.

[0033] The copper-iron alloy wire of the present invention has a high-temperature softening temperature of above 600°C, high resistance to high-temperature corrosion, a penetration of less than 0.01 mm at 750°C for 60 minutes, and a friction coefficient of less than 0.2 (for steel), and is more suitable for preparing electric iron cores. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a structural schematic diagram of the crystallizer of the present invention.

[0035] Figure 2 This is the metallographic H-1000× image of the copper-iron alloy wire of Example 1.

[0036] Figure 3 This is the metallographic Z-1000× image of the copper-iron alloy wire of Example 1.

[0037] Figure 4 This is the metallographic H-1000× image of the copper-iron alloy wire of Example 2.

[0038] Figure 5 This is the metallographic Z-1000× image of the copper-iron alloy wire of Example 2.

[0039] Figure 6 This is the metallographic H-1000× image of the copper-iron alloy wire of Comparative Example 1.

[0040] Figure 7 This is the metallographic Z-1000× image of the copper-iron alloy wire of Comparative Example 1.

[0041] Figure 8 This is the metallographic H-500× image of the copper wire of Comparative Example 2.

[0042] Fig. 9 This is the metallographic Z-500× image of the copper wire of Comparative Example 2. DETAILED DESCRIPTION

[0043] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments, but is not intended to be limiting of the present invention. It should be noted that the embodiments and features in the embodiments of the present invention may be combined with each other without conflict.

[0044] Example 1

[0045] This embodiment provides a specification of The specific production process of the electric iron core is as follows:

[0046] The raw materials are weighed according to the following mass ratio: Fe 20%, Ni 0.8%, Cr 0.3%, and the balance is Cu and other impurity elements that need to be controlled.

[0047] Step A, smelting is carried out in a 300kg medium frequency horizontal continuous casting furnace, power is turned on, electrolytic nickel is first added into the furnace, and then the electrolytic copper plate is added. After the electrolytic plate is melted, the temperature is set at 1280°C, and the pure iron block is added. During the process of adding pure iron, charcoal needs to be used for covering, and the covering thickness is more than 100mm. Activated carbon needs to be added at the same time as the charcoal is added. After the pure iron is added and melted, it is kept warm at 1180°C for 1.5h, and then the temperature is raised to 1380°C for 2h. After the insulation is completed, it is finally kept warm at 1520°C for 1h. After three stages of insulation, the temperature is adjusted to 1400°C, copper-chromium intermediate alloy is added, covered with 200mm charcoal, the crystallizer is assembled, and an electromagnetic stirring device is installed.

[0048] Step B, after completing the smelting process, start continuous casting production, the specifications are The traction speed is 200mm / min, the temperature is 1380℃, the inlet and outlet temperature difference of cooling water is 60℃, and the electromagnetic stirring frequency is 20HZ. After the parameters are set, traction begins.

[0049] refer to Figure 1 In this embodiment, a strong cooling crystallizer is used to quickly obtain highly saturated and evenly mixed copper and iron materials. In order to ensure that copper and iron do not have significant stratification problems, the cooling intensity of the crystallizer must be strengthened. The specific structure of the crystallizer is as follows:

[0050] It includes: graphite sleeve 6, electromagnetic stirring area, primary cooling area and secondary cooling area;

[0051] The graphite sleeve 6 passes through the electromagnetic stirring area and the primary cooling area in sequence, and the outlet of the graphite sleeve 6 faces the secondary cooling area;

[0052] The electromagnetic stirring region includes: a thermal insulation layer 4 and an electromagnetic stirrer 5, wherein the thermal insulation layer 4 is arranged outside the graphite sleeve 6, and the electromagnetic stirrer 5 is arranged outside the thermal insulation layer 4;

[0053] The primary cooling area includes: a copper sleeve 14, an iron sleeve 15, a laminar cooling zone 2, a water inlet 1 and a water outlet 3, the copper sleeve 14 is arranged on the outside of the graphite sleeve 6, the laminar cooling zone 2 is arranged between the copper sleeve 14 and the iron sleeve 15, and the water inlet 1 and the water outlet 2 are connected to the laminar cooling zone 2;

[0054] The secondary cooling area includes: a first water chamber 7, a second water chamber 8, a third water chamber 8, a cooling water separation pipe 11, and a second cooling water chamber 12. The first water chamber 7, the second water chamber 8, and the third water chamber 5 are sequentially arranged on the outside of the passage area of ​​the copper rod to be cooled. The first water chamber 7, the second water chamber 8, and the third water chamber 9 respectively have water rings 10, and the copper rod to be cooled passes through the three water rings in sequence. At the same time, the first water chamber 7, the second water chamber 8, and the third water chamber 9 are respectively connected to the second cooling water chamber 12 through the cooling water separation pipe 11.

[0055] The working principle of the above-mentioned strong cooling crystallizer is as follows:

[0056] Electromagnetic stirring part: The copper and iron liquid begins to enter the graphite sleeve 6. Due to the presence of the insulation layer 4 in this area, it will not solidify quickly, but will mix the alloy components under the action of electromagnetic stirring to avoid the occurrence of stratification. Solidification part: When traction begins, water starts to flow into the water inlet 1. After the water flows in, the water flows directly into the laminar cooling zone 2 for heat exchange, and takes away the heat through the fast and stable laminar flow zone. This part is used to quickly solidify the copper and iron liquid. Secondary cooling area: When the copper and iron rods enter this area, there will be a three-gradient cooling water ring to provide a temperature gradient to the axial area of ​​the copper rod for a cold zone, thereby refining the grains, increasing the axial grains, and avoiding the appearance of coarse columnar dendrites, thereby achieving a uniform composition while also assisting in refining the structure, so that the strength, hardness and plasticity of the material are improved.

[0057] Step C: put the continuous cast copper and iron bars into a trolley furnace, heat them to 950°C, and keep them warm for 50 minutes. After heating, use a groove rolling mill to roll them to

[0058] Step D, the rolled wire is drawn (annealed) to a predetermined bottom specification wire by a straight drawing machine,

[0059] Step E: The hardened wire needs to be bright pickled.

[0060] Step F: Straightening is required after annealing, with a straightness of 0.5mm / 2m.

[0061] Step G: The straightened wire is subjected to bright aging annealing treatment at 530°C + 2h.

[0062] Step H: After the precision inspection is completed, it can be put into storage.

[0063] The copper-iron alloy wire produced according to the above method can obtain a high-temperature softening temperature of 680°C, has a high resistance to high-temperature corrosion, 750°C, 60min, the penetration reaches 0.005mm, the friction coefficient is 0.1 (for steel), and the soldering service life of the electric iron head is significantly improved.

[0064] refer to Figure 2-3 It can be seen that the main phases are matrix Cu phase + Fe phase + trace Cr3Ni2 phase and Ni phase. A large amount of evenly distributed Fe-rich phase can form dislocation aggregation points in the material deformation process, increase the strength and hardness of the material. Due to the strengthening effect of the iron phase on the material, the annealing softening temperature continues to increase, and the wear resistance of the material is also improved, especially for the stability under high temperature. The trace particle phase Cr3Ni2 phase and Ni phase can stabilize the corrosion resistance and wear resistance of the material.

[0065] Example 2

[0066] This embodiment provides a specification of The specific production process of the electric iron core is as follows:

[0067] The raw materials are weighed according to the following mass ratio: Fe 40%, Ni 0.5%, Cr 0.2%, and the balance is Cu and other impurity elements that need to be controlled.

[0068] Step A, smelting is carried out in a 300kg medium frequency horizontal continuous casting furnace, power is turned on, electrolytic nickel is first added into the furnace, and then the electrolytic copper plate is added. After the electrolytic plate is melted, the temperature is set at 1300°C, and the pure iron block is added. During the process of adding pure iron, charcoal needs to be used for covering, and the covering thickness is more than 100mm. Activated carbon needs to be added at the same time as the charcoal is added. After the pure iron is added and melted, it is kept warm at 1200°C for 3h, and then the temperature is increased to 1400°C for 3h. After the insulation is completed, it is finally kept warm at 1580°C for 2h. After three stages of insulation, the temperature is adjusted to 1450°C, copper-chromium intermediate alloy is added, covered with 200mm charcoal, the crystallizer is assembled, and an electromagnetic stirring device is installed.

[0069] Step B, after the smelting process is completed, the strong cooling crystallizer described in Example 1 is used to start continuous casting production, with specifications of The traction speed is 180mm / min, the temperature is 1480℃, the inlet and outlet temperature difference of cooling water is 80℃, and the electromagnetic stirring frequency is 40HZ. After the parameters are set, traction begins.

[0070] Step C: put the continuous cast copper and iron bars into a trolley furnace, heat them to 980°C, and keep them warm for 60 minutes. After heating, use a groove rolling mill to roll them into

[0071] Step D: The rolled wire is drawn (annealed) to a predetermined bottom specification wire by a straight drawing machine.

[0072] Step E: The work-hardened wire needs to be bright pickled.

[0073] Step F: Straightening is required after annealing, with a straightness of 0.5mm / 2m.

[0074] Step G: The straightened wire is subjected to bright aging annealing treatment at 550°C + 4h.

[0075] Step H: After the precision inspection is completed, it can be put into storage.

[0076] The copper-iron alloy wire produced according to the above method can obtain a high-temperature softening temperature of 750°C, has a high resistance to high-temperature corrosion, 750°C, 60min, the penetration reaches 0.005mm, the friction coefficient is 0.05 (for steel), and the soldering service life of the electric iron head is significantly improved.

[0077] refer to Figure 4-5It can be seen that the main phases are matrix Cu phase + Fe phase + trace Cr3Ni2 phase and Ni phase. A large amount of evenly distributed Fe-rich phase can form dislocation aggregation points in the material deformation process, increase the strength and hardness of the material. Due to the strengthening effect of the iron phase on the material, the annealing softening temperature continues to increase, and the wear resistance of the material is also improved, especially for the stability under high temperature. The trace particle phase Cr3Ni2 phase and Ni phase can stabilize the corrosion resistance and wear resistance of the material.

[0078] Comparative Example 1

[0079] This comparative example provides a specification of The specific production process of the electric iron core is as follows:

[0080] The raw materials are weighed according to the following mass ratio: Fe 20%, Ni 0.8%, Cr 0.3%, and the balance is Cu and other impurity elements that need to be controlled.

[0081] Step A, smelting is carried out in a 300kg medium frequency horizontal continuous casting furnace, power is turned on, electrolytic copper plates and electrolytic nickel are added, and after the electrolytic plates are melted, the temperature is set at 1380°C, pure iron blocks and copper-chromium intermediate alloys are added, and during the process of adding pure iron, charcoal covering is required, and the covering thickness is more than 100mm.

[0082] Step B, after completing the smelting process, use a common crystallizer to start continuous casting production, the specifications are The traction speed is 200mm / min, the temperature is 1380℃, and the temperature difference between the inlet and outlet of the cooling water is 40℃. After the parameters are set, traction begins.

[0083] Step C, putting the drawn continuous cast copper and iron bars into a trolley furnace, heating them to 980°C, keeping them warm for 60 minutes, and extending them using a straight pulling car after heating.

[0084]

[0085] Step E: The hardened wire needs to be bright pickled

[0086] Step F: Straightening is required after annealing, with a straightness of 0.5mm / 2m.

[0087] Step G: The straightened wire is subjected to bright aging annealing treatment at 530°C + 2h.

[0088] Step H: After the fine inspection is completed, it can be put into storage.

[0089] The copper-iron alloy wire produced according to the above method can obtain a high temperature softening temperature of 750℃ / 250℃ / 550℃, and has a low resistance to high temperature corrosion. At 750℃, 60min, the penetration reaches 0.5mm, the friction coefficient is 0.8 (for steel), the soldering service life of the electric iron head is reduced, and the stability is poor.

[0090] refer to Figure 6-7 It can be seen that the main phases are matrix Cu phase + Fe phase + trace Cr3Ni2 phase, Ni phase, and the distributed iron-rich Fe phase is unevenly distributed. There is a serious iron enrichment problem, which can easily cause the high-temperature performance of the material to be very unstable, and the wear resistance and corrosion resistance are weakened.

[0091] Comparative Example 2

[0092] This comparative example provides a specification of The specific production process of the electric iron core is as follows: the composition is red copper, and other impurity elements that need to be controlled.

[0093] Step A: The specific smelting is carried out in a 300kg medium frequency horizontal continuous casting furnace. The power is turned on and an electrolytic plate is added into the furnace. After the electrolytic plate is melted, the temperature is set at 1200°C and the charcoal covering thickness is above 100mm.

[0094] Step B, after completing the smelting process, use a common crystallizer to start continuous casting production, the specifications are The traction speed is 250mm / min, the temperature is 1280℃, the inlet and outlet temperature difference of cooling water is 40℃, and the water pressure is 0.4Mpa. After the parameters are set, traction begins.

[0095] Step C, extending the drawn continuous casting bars by using a straight pulling car.

[0096]

[0097] Step E: The work-hardened wire needs to be bright pickled.

[0098] Step F: Straightening is required after annealing, with a straightness of 0.5mm / 2m.

[0099] Step H: After the precision inspection is completed, it can be put into storage.

[0100] The copper wire produced according to the above method can obtain a high temperature softening temperature of 350°C, has a low resistance to high temperature corrosion, 750°C, 60min, the penetration reaches 0.3mm, the friction coefficient is 0.6 (for steel), the soldering service life of the electric iron head is general, and the core head needs to be replaced frequently.

[0101] refer to Figure 8-9 It can be seen that the main phase is the matrix Cu phase.

[0102] The properties of the wires prepared in the above Examples 1-2 and Comparative Examples 1-2 are shown in Table 1 below:

[0103] Table 1

[0104]

[0105] The above description is only a preferred embodiment of the present invention, and does not limit the implementation mode and protection scope of the present invention. For those skilled in the art, it should be aware that all solutions obtained by equivalent substitutions and obvious changes made using the contents of the specification and illustrations of the present invention should be included in the protection scope of the present invention.

Claims

1. A copper-iron alloy wire, characterized in that: The invention comprises the following components in mass percentage: Fe 20%-50%, and Cu balance.

2. The copper-iron alloy wire according to claim 1, characterized in that: Also includes Ni 0.5%-1.0%, Cr 0.1%-0.5%.

3. The copper-iron alloy wire according to claim 2, characterized in that: The copper-iron alloy comprises a matrix Cu phase, a Fe phase, a Cr phase, a Fe-Cr phase and a trace amount of Cr3Ni2 phase; wherein the Cr particle size is 5-20 μm, the Cr particle size / Fe particle size is less than 1, and the Fe phase / Cr phase is greater than 200.

4. The method for preparing the copper-iron alloy wire according to any one of claims 1 to 3, characterized in that: The steps include: Melting - horizontal continuous casting - hot rolling - wire drawing, straightening - aging annealing; Among them, smelting: adopts multi-gradient graded insulation treatment.

5. The method for preparing the copper-iron alloy wire according to claim 4, characterized in that: The multi-gradient graded thermal insulation treatment has three or more gradients.

6. The method for preparing the copper-iron alloy wire according to claim 5, characterized in that: The multi-gradient graded insulation treatment specifically adopts a three-stage melting and insulation process: the raw materials are added to the melting furnace, and after melting, the temperature is kept at 1150-1200°C for 1-3h, and then the temperature is increased to 1350°C-1400°C for 1-3h. After the insulation is completed, 1520°C-1580°C is used for insulation for 1-2h. After three stages of insulation, copper-chromium intermediate alloy is added, the crystallizer is assembled, the electromagnetic stirring device is put on, and traction is started.

7. The method for preparing the copper-iron alloy wire according to claim 6, characterized in that: The specific process of adding the raw materials is as follows: electrolytic nickel and electrolytic copper plates are added into the continuous casting furnace, and after melting, the temperature is set at 1250° C.-1300° C. and then pure iron blocks are added.

8. The method for preparing the copper-iron alloy wire according to claim 4, characterized in that: The specific parameters in the horizontal continuous casting process are set as follows: temperature 1350℃-1400℃, cooling water inlet and outlet temperature difference 60-80℃, electromagnetic stirring frequency 20HZ-50HZ.

9. The method for preparing the copper-iron alloy wire according to claim 4, characterized in that: The horizontal continuous casting process uses a strong cooling crystallizer, which includes a graphite sleeve, an electromagnetic stirring area, a primary cooling area and a secondary cooling area; The graphite sleeve passes through the electromagnetic stirring area and the primary cooling area in sequence, and the outlet of the graphite sleeve faces the secondary cooling area; The electromagnetic stirring region comprises: a thermal insulation layer and an electromagnetic stirrer, wherein the thermal insulation layer is arranged outside the graphite sleeve, and the electromagnetic stirrer is arranged outside the thermal insulation layer; The primary cooling area adopts laminar cooling method; The secondary cooling area adopts a cooling method with three gradients.

10. The method for preparing the copper-iron alloy wire according to claim 9, characterized in that: The primary cooling area includes: a copper sleeve, an iron sleeve, a laminar cooling zone, a water inlet and a water outlet, the copper sleeve is arranged outside the graphite sleeve, the laminar cooling zone is arranged between the copper sleeve and the iron sleeve, and the water inlet and the water outlet are connected to the laminar cooling zone; The secondary cooling area includes: a first water chamber, a second water chamber, a third water chamber, a cooling water distribution pipe, and a second cooling water chamber. The first water chamber, the second water chamber, and the third water chamber are sequentially arranged on the outside of the passage area of ​​the copper rod to be cooled. The first water chamber, the second water chamber, and the third water chamber respectively have water rings, and the copper rod to be cooled passes through three water rings in sequence. At the same time, the first water chamber, the second water chamber, and the third water chamber are respectively connected to the second cooling water chamber through the cooling water distribution pipe.

11. Use of the copper-iron alloy wire according to any one of claims 1 to 3 in preparing an electric iron core.

Citation Information

Cited By

  • High-strength and high-conductivity copper-tin alloy wire resistant to high-temperature softening and preparation process thereof

    CN119530605A

  • High-strength high-conductivity copper-tin alloy wire resistant to high-temperature softening and a preparation process thereof

    CN119530605B