Copper-zinc-tin-based strained glass single crystal alloy

Through the preparation method of copper-zinc-tin-based strained glass single crystal alloy, the process flow is simplified by using annealing and quenching processes, the problems of brittle fracture and high-cost preparation of Cu-based polycrystalline alloy are solved, and Cu-based strain with unique functional characteristics is achieved The low-cost and efficient preparation of glass single crystal alloys has expanded its application areas.

CN118880104APending Publication Date: 2024-11-01SHENZHEN RES INST OF XIAMEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410928598.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing Cu-based polycrystalline alloys are prone to brittle fracture along the grain boundary direction when loading large stresses. The traditional method of preparing single crystals is expensive and the process is cumbersome, which limits its use in practical applications.

Method used

Using the preparation method of copper-zinc-tin-based strained glass single crystal alloy, a single crystal alloy with strained glass transition characteristics was obtained by annealing a single phase zone between 700°C and 780°C in a polycrystal cast alloy. The method includes preparing the cast alloy and performing multiple melting and annealing treatments at high temperatures, simplifying the process flow and reducing costs.

Benefits of technology

Achieve low-cost and efficient acquisition of Cu-based strained glass single crystal alloy, with wide temperature domain, small thermal hysteresis, low stress hysteresis, shape memory effect and superelasticity, which broadens its performance in aerospace, military industry and other fields. Application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880104A_ABST
    Figure CN118880104A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of metal single crystal alloy materials, and particularly discloses a copper-zinc-tin-based strain glass single crystal alloy which comprises the following components in percentage by mass: 58-72 wt% of copper, 15-22 wt% of zinc, 13-15 wt% of tin, 0-3 wt% of iron and 0-3 wt% of manganese. A Cu-based alloy system is adopted, the cost is only one tenth of that of a Ti-Ni-based memory alloy which is most widely applied at present, and the Cu-based memory alloy has great application prospects in many fields; the as-cast alloy obtained through smelting can be subjected to strain glass transition after annealing heat treatment, a strain glass alloy material with the peculiar properties of wide temperature range, small heat stagnation, low stress hysteresis, shape memory effect, superelasticity and the like is generated, and compared with a traditional shape memory alloy, the shape memory alloy has unique advantages; the method has special application scenes in many fields such as aerospace, military industry and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal single crystal alloy materials, and in particular to a copper-zinc-tin based strained glass single crystal alloy. Background Art

[0002] Strain glass was first developed in the martensitic system Ti 50-x Ni 50+x It was found that when x is below a certain critical value x c When x exceeds the critical value x, the system will undergo a martensitic phase transition, that is, the parent phase lattice undergoes a long-range shear transformation to a long-range ordered martensite. The response of its crystal structure to stress and temperature leads to functional properties such as shape memory effect and superelasticity. However, when x exceeds the critical value x c When x exceeds the critical value x, there is no martensitic phase transformation in the system, but the alloy still has excellent superelasticity and shape memory effect. c When the temperature rises, the system undergoes another non-martensitic transformation, the strain glass transition. The strain glass transition process is a process of dynamic freezing of local lattice strain, and nanoscale martensitic domains are generated in the parent phase. It is these microstructures that give strain glass unique properties such as wide temperature range, small thermal hysteresis, low stress hysteresis, shape memory effect and superelasticity (Sarkar S, Ren X, Otsuka K. Evidence for strainglass in the ferroelastic-martensitic system Ti (50-x) Ni (50+x) [J]. Phys Rev Lett, 2005, 95(20): 205702). Therefore, strain glass has great application prospects in many fields such as aerospace, medical health, and military industry.

[0003] Among the existing alloy systems, the cost of Cu-based alloys is low, about one-tenth of that of Ni-Ti-based memory alloys, and Cu-based alloys have good processing performance and electrical and thermal conductivity. However, when a large stress is applied to a Cu-based polycrystalline alloy, due to the large difference in strain between grains in different orientations, in order to maintain the strain continuity on the interface, stress concentration will occur at the grain boundary, resulting in fracture along the grain boundary in the alloy. Some Cu-based polycrystalline alloys will experience brittle fracture at a strain of 2%-3%. Therefore, the preparation of Cu-based single crystal alloys is particularly critical for the application of Cu-based alloys. The traditional method of preparing single crystals by directional solidification has high equipment costs and cumbersome processes. In 2016, Japanese scholars Omori et al. prepared large-sized single crystals in the iron-manganese-zinc-tin quaternary alloy system by using a multiple-cycle heat treatment method (T. Omori, H. Iwaizako, R. Kainuma, Abnormal grain growth induced by cyclic heat treatment in Fe-Mn-Al-Ni superelastic alloy, Mater. Des. 101 (2016) 263–269). However, this method of preparing single crystals through a cyclic heat treatment process also has a long cycle, a complicated process, and very strict temperature requirements, which has great limitations in actual production applications.

[0004] Strain glass alloys originate from traditional alloy systems with reversible martensitic phase transformation, but compared with traditional shape memory alloys, they have their own outstanding functional characteristics and unique application scenarios in various fields. The development of strain glass alloys is of great significance for broadening the research and application of shape memory alloys. The field of low-cost and easy-to-process Cu-based strain glass alloys is in the early stages of research. The research on strain glass single crystals has never been reported at home and abroad, and there are still many problems to be solved. For example, the mechanical properties of Cu-based alloys are poor in the polycrystalline state, and brittle fractures are prone to occur along the grain boundary direction. Therefore, obtaining Cu-based strain glass single crystal alloys through simple and effective processes has far-reaching application value. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a copper-zinc-tin based strained glass single crystal alloy.

[0006] In order to achieve the above objectives, one of the technical solutions of the present invention is: a copper-zinc-tin based strained glass single crystal alloy, whose composition in terms of mass percentage includes: 58-72wt% copper, 15-22wt% zinc, 13-15wt% tin, 0-3wt% iron, and 0-3wt% manganese.

[0007] In a preferred embodiment of the present invention, the composition includes, by mass percentage, 60.5-66.5 wt% copper, 18-22 wt% zinc, 13.5-14.5 wt% tin and 2-3 wt% iron.

[0008] In a preferred embodiment of the present invention, the composition includes, by mass percentage, 60-68wt% copper, 15-20wt% zinc, 13.5-14.5wt% tin, 2-3wt% iron, and 1.5-2.5wt% manganese.

[0009] In a preferred embodiment of the present invention, the copper-zinc-tin based strained glass single crystal alloy is obtained by annealing a polycrystalline cast alloy in a single phase region at 700° C.-780° C.

[0010] The second technical solution of the present invention is: a method for preparing a copper-zinc-tin based strained glass single crystal alloy, comprising the following steps:

[0011] (1) preparing a cast alloy 1: copper, Cu65Sn35 master alloy, zinc, iron and manganese are weighed respectively according to their mass percentage compositions, iron, Cu65Sn35 master alloy and manganese are first smelted in an arc melting furnace, and then cooled to obtain a cast alloy 1;

[0012] (2) preparing cast alloy 2: cutting the cast alloy 1 obtained in step (1) into pieces, vacuum-sealing it with copper and zinc in a quartz glass tube for smelting to obtain cast alloy 2;

[0013] (3) The cast alloy 2 obtained in step (2) is annealed in a high-temperature single-phase region and then quenched to obtain a copper-zinc-tin based strained glass single crystal alloy material.

[0014] In a preferred embodiment of the present invention, the smelting times in step (2) is 2-4 times.

[0015] In a preferred embodiment of the present invention, the smelting temperature in step (2) is 1100-1120°C.

[0016] In a preferred embodiment of the present invention, the annealing temperature in step (3) is 700-780° C., and the annealing time is 45-50 h.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] 1. Alloy cost: The present invention adopts a Cu-based alloy system, the cost of which is only one tenth of the most widely used Ti-Ni-based memory alloy, and has great application prospects in many fields;

[0019] 2. Heat treatment method: The traditional method of preparing single crystals by directional solidification, multiple cycles of heat treatment, etc. has high equipment cost and complex process. However, the present invention only needs to keep the alloy in the β single phase region for a period of time and then quench it to obtain a single crystal alloy. The method is simple, efficient and low cost.

[0020] 3. Functional characteristics: Within the composition range of the present invention, the cast alloy obtained by melting will undergo a strain glass transition after annealing heat treatment, producing a strain glass alloy material with unique properties such as a wide temperature range, small thermal hysteresis, low stress hysteresis, shape memory effect and superelasticity. Compared with traditional shape memory alloys, it has unique advantages and has special application scenarios in many fields such as aerospace, military industry and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The microstructure diagrams of the cast alloy and the quenched alloy in Example 5 of the present invention;

[0022] Figure 2 The photos are of the cast alloy in Example 5 of the present invention and the quenched alloy with large grains of about 13 mm in diameter and about 35 mm in length obtained by heat treatment at 750° C. for 48 hours;

[0023] Figure 3 The microstructure diagrams of the cast alloy and the quenched alloy in Example 10 of the present invention;

[0024] Figure 4 The photos are of the cast alloy in Example 10 of the present invention and the alloy with large grains of about 13 mm in diameter and about 35 mm in length obtained by heat treatment at 730° C. for 48 hours;

[0025] Figure 5 The resistance-temperature characteristic curve of Example 5 of the present invention can be confirmed to be a strained glass alloy;

[0026] Figure 6 The resistance-temperature characteristic curve of Example 10 of the present invention can be confirmed to be a strained glass alloy;

[0027] Figure 7 The stress-strain curve of Example 5 of the present invention shows that it has excellent superelasticity;

[0028] Figure 8 This is the stress-strain curve of Example 10 of the present invention, which shows that it has excellent superelasticity. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is described in more detail below with reference to the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited to these embodiments.

[0030] A copper-zinc-tin based strained glass single crystal alloy comprises, by mass percentage, 58-72wt% copper, 15-22wt% zinc, 13-15wt% tin, 0-3wt% iron and 0-3wt% manganese.

[0031] The composition includes, by mass percentage, 60.5-66.5 wt % of copper, 18-22 wt % of zinc, 13.5-14.5 wt % of tin and 2-3 wt % of iron.

[0032] The composition includes, by mass percentage, 60-68wt% copper, 15-20wt% zinc, 13.5-14.5wt% tin, 2-3wt% iron, and 1.5-2.5wt% manganese.

[0033] The copper-zinc-tin-based strained glass single crystal alloy is obtained by annealing a polycrystalline cast alloy in a single phase region at 700° C.-780° C.

[0034] A method for preparing a copper-zinc-tin based strained glass single crystal alloy comprises the following steps:

[0035] (1) preparing a cast alloy 1: copper, Cu65Sn35 master alloy, zinc, iron and manganese are weighed respectively according to their mass percentage compositions, iron, Cu65Sn35 master alloy and manganese are first smelted in an arc melting furnace, and then cooled to obtain a cast alloy 1;

[0036] (2) preparing cast alloy 2: cutting the cast alloy 1 obtained in step (1) into pieces, vacuum-sealing it with copper and zinc in a quartz glass tube for smelting to obtain cast alloy 2;

[0037] (3) The cast alloy 2 obtained in step (2) is annealed in a single phase region at a high temperature of 700° C. to 780° C., and then quenched to obtain a copper-zinc-tin based strained glass single crystal alloy material.

[0038] The smelting times in the step (2) is 2-4 times.

[0039] The smelting temperature in step (2) is 1100-1120°C.

[0040] In the step (3), the annealing temperature is 700-780° C. and the annealing time is 45-50 hours.

[0041] Example 1

[0042] Copper, zinc, Cu65Sn35 master alloy and iron metal raw materials are weighed according to the mass percentage of copper 39%, zinc 18.5%, Cu65Sn35 master alloy 40% and iron 2.5%, respectively; the Cu65Sn35 master alloy and iron are first smelted in an electric arc furnace, and the smelting is repeated 3 times to ensure uniformity, and a cast alloy 1 is obtained after cooling; the cast alloy 1 obtained above is cut into pieces and vacuum-sealed in a quartz tube with copper and zinc, and smelted at 1100°C in a pit furnace to obtain a cast alloy 2; the cast alloy 2 obtained above is annealed at 750°C for 48 hours, and then quenched with ice water to obtain a copper-zinc-tin based strain glass single crystal alloy material.

[0043] Example 2

[0044] Copper, zinc, Cu65Sn35 master alloy and iron metal raw materials are weighed according to the mass percentage of copper 38.5%, zinc 19%, Cu65Sn35 master alloy 40% and iron 2.5%, respectively. The Cu65Sn35 master alloy and iron are first smelted in an electric arc furnace, and the smelting is repeated 3 times to ensure uniformity. After cooling, a cast alloy 1 is obtained; the cast alloy 1 obtained above is cut into pieces and vacuum-sealed in a quartz tube with copper and zinc, and then smelted at 1100°C in a pit furnace to obtain a cast alloy 2; then the cast alloy 2 is annealed at 750°C for 48 hours, and then quenched with ice water to obtain a copper-zinc-tin based strain glass single crystal alloy material.

[0045] Example 3

[0046] Copper, zinc, Cu65Sn35 master alloy and iron metal raw materials are weighed according to the mass percentage of copper 38%, zinc 19.5%, Cu65Sn35 master alloy 40% and iron 2.5%, respectively; the Cu65Sn35 master alloy and iron are first smelted in an electric arc furnace, and the smelting is repeated 3 times to ensure uniformity, and a cast alloy 1 is obtained after cooling; the cast alloy 1 obtained above is cut into pieces and vacuum-sealed in a quartz tube with copper and zinc, and smelted at 1100° C. in a pit furnace to obtain a cast alloy 2; the cast alloy 2 is then annealed at 730° C. for 48 hours, and then quenched with ice water to obtain a copper-zinc-tin-based strain glass single crystal alloy material.

[0047] Example 4

[0048] Copper, zinc, Cu65Sn35 master alloy and iron metal raw materials are weighed according to the mass percentage of copper 37.5%, zinc 20%, Cu65Sn35 master alloy 40% and iron 2.5%, respectively; the Cu65Sn35 master alloy and iron are first smelted in an electric arc furnace, and the smelting is repeated 3 times to ensure uniformity, and a cast alloy 1 is obtained after cooling; the cast alloy 1 obtained above is cut into pieces and vacuum-sealed in a quartz tube with copper and zinc, and smelted at 1100° C. in a pit furnace to obtain a cast alloy 2; the cast alloy 2 is then annealed at 730° C. for 48 hours, and then quenched with ice water to obtain a copper-zinc-tin based strain glass single crystal alloy material.

[0049] Example 5

[0050] Copper, zinc, Cu65Sn35 master alloy and iron metal raw materials are weighed according to the mass percentage of copper 36.5%, zinc 21%, Cu65Sn35 master alloy 40% and iron 2.5%, respectively. The Cu65Sn35 master alloy and iron are first smelted in an electric arc furnace, and the smelting is repeated 3 times to ensure uniformity. After cooling, a cast alloy 1 is obtained; the cast alloy 1 obtained above is cut into pieces and vacuum-sealed in a quartz tube with copper and zinc, and then smelted at 1100°C in a pit furnace to obtain a cast alloy 2; then the cast alloy 2 is annealed at 730°C for 48 hours, and then quenched with ice water to obtain a copper-zinc-tin based strain glass single crystal alloy.

[0051] Its grain microstructure and macroscopic pictures are as follows Figure 1 and 2 As shown in the figure, it can be seen that a single crystal was obtained by a one-step heat treatment at 750℃ for 48h. Its temperature-resistivity curve is shown in Figure 5 As shown, it shows the characteristics of strain glass, and its stress-strain curve is as follows Figure 7 As shown, it shows that it has excellent superelasticity.

[0052] Example 6

[0053] Copper, zinc, Cu65Sn35 master alloy and iron metal raw materials are weighed according to the mass percentage of copper 39.5%, zinc 16%, Cu65Sn35 master alloy 40%, iron 2.5% and manganese 2% respectively. The Cu65Sn35 master alloy, iron and manganese are first smelted in an electric arc furnace, and the smelting is repeated 3 times to ensure uniformity. After cooling, a cast alloy 1 is obtained; the cast alloy 1 obtained above is cut into pieces and vacuum-sealed in a quartz tube with copper and zinc, and then smelted at 1120°C in a pit furnace to obtain a cast alloy 2; then the cast alloy 2 is annealed at 750°C for 48 hours, and then quenched with ice water to obtain a copper-zinc-tin based strain glass single crystal alloy material.

[0054] Example 7

[0055] Copper, zinc, Cu65Sn35 master alloy and iron metal raw materials are weighed according to the mass percentage of copper 38%, zinc 17.5%, Cu65Sn35 master alloy 40%, iron 2.5% and manganese 2% respectively. The Cu65Sn35 master alloy, iron and manganese are first smelted in an electric arc furnace, and the smelting is repeated 3 times to ensure uniformity. After cooling, a cast alloy 1 is obtained; the cast alloy 1 obtained above is cut into pieces and vacuum-sealed in a quartz tube with copper and zinc, and then smelted at 1120° C. in a pit furnace to obtain a cast alloy 2; then the cast alloy 2 is annealed at 730° C. for 48 hours, and then quenched with ice water to obtain a copper-zinc-tin-based strain glass single crystal alloy material.

[0056] Example 8

[0057] Copper, zinc, Cu65Sn35 master alloy and iron metal raw materials are weighed according to the mass percentage of copper 37.5%, zinc 18%, Cu65Sn35 master alloy 40%, iron 2.5% and manganese 2% respectively. The Cu65Sn35 master alloy, iron and manganese are first smelted in an electric arc furnace, and the smelting is repeated 3 times to ensure uniformity. After cooling, a cast alloy 1 is obtained; the cast alloy 1 obtained above is cut into pieces and vacuum-sealed in a quartz tube with copper and zinc, and then smelted at 1100° C. in a pit furnace to obtain a cast alloy 2; then the cast alloy 2 is annealed at 730° C. for 48 hours, and then quenched with ice water to obtain a copper-zinc-tin-based strain glass single crystal alloy material.

[0058] Example 9

[0059] Copper, zinc, Cu65Sn35 master alloy and iron metal raw materials are weighed according to the mass percentage of copper 37%, zinc 18.5%, Cu65Sn35 master alloy 40%, iron 2.5% and manganese 2% respectively. The Cu65Sn35 master alloy, iron and manganese are first smelted in an electric arc furnace, and the smelting is repeated 3 times to ensure uniformity. After cooling, a cast alloy 1 is obtained; the cast alloy 1 obtained above is cut into pieces and vacuum-sealed in a quartz tube with copper and zinc, and then smelted at 1100° C. in a pit furnace to obtain a cast alloy 2; then the cast alloy 2 is annealed at 730° C. for 48 hours, and then quenched with ice water to obtain a copper-zinc-tin-based strain glass single crystal alloy material.

[0060] Example 10

[0061] Copper, zinc, Cu65Sn35 master alloy and iron metal raw materials are weighed according to the mass percentage of copper 36.5%, zinc 19%, Cu65Sn35 master alloy 40%, iron 2.5% and manganese 2% respectively. The Cu65Sn35 master alloy, iron and manganese are first smelted in an electric arc furnace, and the smelting is repeated 3 times to ensure uniformity. After cooling, a cast alloy 1 is obtained; the cast alloy 1 obtained above is cut into pieces and vacuum-sealed in a quartz tube with copper and zinc, and then smelted at 1100° C. in a pit furnace to obtain a cast alloy 2; then the cast alloy 2 is annealed at 730° C. for 48 hours, and then quenched with ice water to obtain a copper-zinc-tin-based strain glass single crystal alloy material.

[0062] Its grain microstructure and macroscopic pictures are as follows Figure 3 and 4 As shown in the figure, it can be seen that a single crystal was obtained by a one-step heat treatment at 730℃ for 48h. Its temperature-resistivity curve is shown in Figure 6 As shown, it shows the characteristics of strain glass. Its stress-strain curve is as follows Figure 8 As shown, it shows that it has excellent superelasticity.

[0063] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A copper-zinc-tin based strained glass single crystal alloy, characterized in that: The composition thereof includes, by mass percentage, 58-72wt% copper, 15-22wt% zinc, 13-15wt% tin, 0-3wt% iron, and 0-3wt% manganese.

2. The copper-zinc-tin based strained glass single crystal alloy according to claim 1, characterized in that: The composition thereof includes, by mass percentage, 60.5-66.5wt% of copper, 18-22wt% of zinc, 13.5-14.5wt% of tin and 2-3wt% of iron.

3. The copper-zinc-tin based strained glass single crystal alloy according to claim 1, characterized in that: The composition thereof includes, by mass percentage, 60-68wt% copper, 15-20wt% zinc, 13.5-14.5wt% tin, 2-3wt% iron, and 1.5-2.5wt% manganese.

4. The copper-zinc-tin based strained glass single crystal alloy according to claim 1, characterized in that: The copper-zinc-tin-based strained glass single crystal alloy is obtained by annealing a polycrystalline cast alloy in a single phase region at 700° C.-780° C.

5. A method for preparing the copper-zinc-tin based strained glass single crystal alloy according to any one of claims 1 to 4, characterized in that: The steps include: (1) preparing a cast alloy 1: copper, Cu65Sn35 master alloy, zinc, iron and manganese are weighed respectively according to their mass percentage compositions, iron, Cu65Sn35 master alloy and manganese are first smelted in an arc melting furnace, and then cooled to obtain a cast alloy 1; (2) preparing cast alloy 2: cutting the cast alloy 1 obtained in step (1) into pieces, vacuum-sealing it with copper and zinc in a quartz glass tube for smelting to obtain cast alloy 2; (3) The cast alloy 2 obtained in step (2) is annealed in a high-temperature single-phase region and then quenched to obtain a copper-zinc-tin based strained glass single crystal alloy material.

6. The method for preparing the copper-zinc-tin based strained glass single crystal alloy according to claim 5, characterized in that: The smelting times in the step (2) is 2-4 times.

7. The method for preparing the copper-zinc-tin based strained glass single crystal alloy according to claim 5, characterized in that: The smelting temperature in step (2) is 1100-1120°C.

8. The method for preparing the copper-zinc-tin based strained glass single crystal alloy according to claim 5, characterized in that: In the step (3), the annealing temperature is 700-780° C. and the annealing time is 45-50 hours.