Aluminum alloy plate with high stability and high bake hardening performance as well as preparation method and application of aluminum alloy plate

By compounding the addition of trace Sn and Cu elements to aluminum alloy sheets and adopting double-stage homogenization and high-temperature solution treatment, the problems of insufficient parking stability and paint performance of existing aluminum alloy sheets at room temperature are solved, and high stability is achieved and high baking hardening performance, suitable for automobile manufacturing, reducing production difficulty and cost.

CN118880122APending Publication Date: 2024-11-01CHINALCO MATERIALS APPL RES INST CO LTD +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410938181.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing aluminum alloy sheets have shortcomings in room temperature parking stability and paint performance, and are difficult to produce industrially and costly, making it difficult to meet the needs of lightweight automobiles.

Method used

By adding trace Sn and Cu elements in composite, and using double-stage homogenization and high-temperature solution treatment, the vacancy and cluster state are regulated, the room temperature parking stability and paint hardening performance of the plate are improved, and aluminum alloy with low yield strength in T4P state is prepared. Plate, suitable for automobile manufacturing.

Benefits of technology

It realizes high stability and high baking and hardening properties of aluminum alloy sheets, reduces material usage, reduces carbon emissions, simplifies production processes, reduces costs, and is suitable for complex parts forming and automobile manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004942066350000061
    Figure BDA0004942066350000061
  • Figure BDA0004942066350000062
    Figure BDA0004942066350000062
  • Figure BDA0004942066350000071
    Figure BDA0004942066350000071
Patent Text Reader

Abstract

The invention discloses an aluminum alloy plate with high stability and high bake hardening performance as well as a preparation method and application of the aluminum alloy plate. The aluminum alloy plate comprises the following components in percentage by mass: 0.20%-1.50% of Si; fe: less than or equal to 0.40%; 0.06% to 0.30% of Cu; 0.05% to 0.2% of Mn; 0.20% to 0.80% of Mg; less than or equal to 0.10% of Cr; 0.01 to 0.05 percent of Ti; sn: 0.005 to 0.045%, and the balance being Al. The components and the preparation process of the aluminum alloy plate are greatly different from those in the prior art, vacancy, cluster and precipitated phase states of the prepared plate are effectively regulated and controlled, so that the room-temperature parking stability and baking varnish hardenability of the plate are greatly improved, and the aluminum alloy plate has low yield strength in a T4P state and high-room-temperature parking stability; and after baking, the T8X-state high baking varnish performance can be achieved, and the method can be widely applied to the automobile industry and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy manufacturing, and in particular to an aluminum alloy plate with high stability and high baking hardening performance, and a preparation method and application thereof. Background Art

[0002] The exhaust emissions from gasoline vehicles are one of the major sources of global air pollution. Lightweighting of automobiles is an important means of energy conservation, emission reduction and pollution reduction. Aluminum alloy sheets are considered to be ideal materials for lightweighting of automobiles due to their light weight, high specific strength and excellent comprehensive performance. At present, 5xxx and 6xxx aluminum alloys are mainly used to prepare automobile sheets. Among them, 6xxx alloy is the most widely used, and there is a trend of further expanding the scope of application and replacing 5xxx aluminum alloy, which is more conducive to recycling.

[0003] In recent years, some domestic universities and research institutes have conducted research on 6xxx aluminum alloy automotive plates, most of which only focus on some performance indicators, and rarely report on Sn and Cu composite microalloying. For example:

[0004] Patent CN 117305670 B improves the performance of baking varnish by adjusting the cooling rate, but does not involve the addition of Sn and Cu composite microalloys.

[0005] Patent CN 107699755 B simultaneously adds trace elements such as Sn and In, and adds a large amount of Zn element to improve the performance of the paint, but increases the cost and difficulty of industrial production.

[0006] Japanese patents JP6301175B2 and JP6190308B2 also use Sn elements to improve the room temperature parking stability and paint performance of the material, but they do not add Cu elements to further improve the paint effect. In addition, the homogenization and solid solution temperatures they use are relatively low. Summary of the invention

[0007] The present invention aims to provide an aluminum alloy plate with high stability and high baking hardening performance, a preparation method and application thereof. The aluminum alloy plate has low yield strength in T4P state, high room temperature parking stability, and high baking paint performance in T8X state after baking.

[0008] In order to achieve the above object, according to one aspect of the present invention, there is provided an aluminum alloy plate with high stability and high bake hardening performance. The aluminum alloy plate comprises the following components by mass percentage: Si: 0.20% to 1.50%; Fe: ≤0.40%; Cu: 0.06-0.30%; Mn: 0.05% to 0.2%; Mg: 0.20% to 0.80%; Cr: ≤0.10%; Ti: 0.01-0.05; Sn: 0.005-0.045%, and the balance Al.

[0009] Furthermore, the aluminum alloy plate is prepared by the following preparation method: (1) casting an aluminum alloy melt ingot; (2) homogenizing the ingot; (3) hot rolling and cold rolling the homogenized ingot in sequence to prepare a cold-rolled coil; (4) solutionizing and quenching the cold-rolled coil to obtain a coil; (5) pre-aging the quenched coil to obtain a T4P state coil; (7) uncoiling, straightening and slicing the T4P state coil after the pre-aging treatment to obtain an aluminum alloy plate.

[0010] Furthermore, the homogenization treatment in step (2) is to heat the mixture to 480-520°C at a rate of 40-70°C / h and keep the temperature for 4-10h, and then heat the mixture to 560-580°C at a rate of 20-40°C / h and keep the temperature for 6-10h.

[0011] Furthermore, the hot rolling start temperature in step (3) is 560-580° C., and the thickness of the hot rolled plate is 4-8 mm.

[0012] Furthermore, in step (3), the thickness of the plate after hot rolling and cold rolling is 0.5-3.0 mm.

[0013] Furthermore, the solution treatment in step (4) is performed in an air cushion continuous annealing furnace, the temperature is raised to 565-585°C at a rate of more than 5°C / s, and kept at this temperature for 0.5-5min, and then cooled to room temperature at a rate of more than 30°C / s.

[0014] Furthermore, the pre-aging treatment in step (5) is carried out in a box-type furnace at 60-90° C. for 4-10 hours.

[0015] Furthermore, the aluminum alloy sheet: the 7-day yield strength of the T4P state sheet is less than 100MPa, and the yield strength increment from 7 days to 180 days is less than 25MPa. The T4P state sheet is pre-stretched by 2% + baked at 185℃ for 20min to obtain the T8X state sheet, the yield strength is greater than 200MPa, and the paint increment is greater than 130MPa.

[0016] According to another aspect of the present invention, there is provided a use of any one of the above-mentioned aluminum alloy sheets with high stability and high bake hardening performance in automobile manufacturing.

[0017] According to another aspect of the present invention, a method for preparing an aluminum alloy plate with high stability and high bake hardening performance is provided. The preparation method comprises: (1) casting an aluminum alloy melt into an ingot; (2) homogenizing the ingot; (3) sequentially hot rolling and cold rolling the homogenized ingot to prepare a cold-rolled coil; (4) performing a solid solution and quenching treatment on the cold-rolled coil to obtain a coil; (5) performing a pre-aging treatment on the quenched coil to obtain a T4P state coil; (7) uncoiling, straightening and slicing the T4P state coil after the pre-aging treatment to obtain an aluminum alloy plate; wherein the aluminum alloy plate comprises the following components by mass percentage: Si: 0.20% to 1.50%; Fe: ≤0.40%; Cu: 0.06-0.30%; Mn: 0.05% to 0.2%; Mg: 0.20% to 0.80%; Cr: ≤0.10%; Ti: 0.01-0.05; Sn: 0.005-0.045%, and the balance Al;

[0018] Preferably, the homogenization treatment in step (2) is to heat the mixture to 480-520°C at a rate of 40-70°C / h and keep the temperature for 4-10h, and then heat the mixture to 560-580°C at a rate of 20-40°C / h and keep the temperature for 6-10h;

[0019] Preferably, the hot rolling start temperature in step (3) is 560-580° C., and the thickness of the hot rolled plate is 4-8 mm;

[0020] Preferably, the thickness of the plate after hot rolling and cold rolling in step (3) is 0.5-3.0 mm;

[0021] Preferably, the solution treatment in step (4) is performed in an air cushion continuous annealing furnace, the temperature is raised to 565-585°C at a rate of 5°C / s or more, and the temperature is kept at this temperature for 0.5-5 min, and the temperature is cooled to room temperature at a rate of 30°C / s or more.

[0022] Preferably, the pre-aging treatment in step (5) is carried out in a box furnace at 50-90° C. for 4-10 h;

[0023] Preferably, the aluminum alloy sheet: the 7-day yield strength of the T4P state sheet is less than 100 MPa, and the yield strength increment from 7 days to 180 days is less than 25 MPa. The T4P state sheet is pre-stretched by 2% + baked at 185℃ for 20 minutes to obtain the T8X state sheet, the yield strength is greater than 200 MPa, and the baking paint increment is greater than 130 MPa.

[0024] The composition and preparation process of the aluminum alloy plate of the present invention are significantly different from those of the prior art. The plate prepared by the present invention effectively regulates the state of vacancies, clusters and precipitation phases, thereby greatly improving the room temperature parking stability and paint hardening of the plate. It has low yield strength in the T4P state, high room temperature parking stability, and high paint hardening performance in the T8X state after baking, and can be widely used in the automotive and other industries.

[0025] Specifically, compared with the prior art, the main differences of the present invention are:

[0026] (1) The present invention adds trace Sn and Cu elements in combination, which not only effectively utilizes the characteristics of Sn elements to bind vacancies and inhibit natural aging, but also combines the characteristics of Cu elements to improve the performance of paint. Compared with the single addition of a certain alloy element, the performance of the sheet is further optimized. By adding trace Sn elements, compared with the main alloying elements Mg and Si in the 6xxx alloy, the Sn element has a stronger vacancy binding ability, thereby binding vacancies and inhibiting the diffusion of Mg and Si elements, greatly improving the room temperature parking stability of the sheet. At the same time, when the Sn element is baked at high temperature, the vacancies are released again, thereby improving the performance of the paint. By adding trace Cu elements, the characteristics of improving the strengthening effect of the paint when baked at high temperature are utilized to further improve the performance of the paint.

[0027] (2) The present invention adopts two-stage homogenization, on the one hand to ensure the effective dissolution of Sn element, and on the other hand to fully consider the actual industrial production. Among them, the use of slow heating fully considers the limitation of equipment capacity during industrial production and the inability to achieve rapid temperature increase. The purpose of the first stage homogenization is to promote the dissolution of the low-melting point phase, increase its melting point and thus increase the temperature of the second stage homogenization. The second stage homogenization temperature needs to reach above 560°C in order to ensure a more complete dissolution of the Sn element, solve the problem of low solubility of the Sn element in aluminum, and avoid overheating and scrapping of the material due to excessive temperature.

[0028] (3) The present invention adopts a high solution temperature to ensure that the Sn element is more fully dissolved, thereby effectively utilizing the properties of the Sn element, while avoiding excessively high temperatures that may cause the material to be overburned and scrapped.

[0029] (4) The present invention only needs to add a very small amount of Sn and Cu elements to significantly improve the stability and paint performance. There is no need to add a large amount of Zn, Cu or expensive elements such as Sc and Zr as in the prior art, and the cost is controllable.

[0030] (5) The present invention does not require additional processes or equipment and can meet the requirements of industrial preparation.

[0031] The technical advancement of the present invention is mainly reflected in:

[0032] (1) The present invention can achieve a T4P state of low yield strength and stable performance of the plate by compositely adding trace amounts of Sn and Cu elements, thereby greatly improving its stamping forming performance and meeting the forming requirements of more complex parts.

[0033] (2) The present invention can achieve higher paint performance after the board is baked by compositely adding trace amounts of Sn and Cu elements, thereby achieving material thinning at equal strength, reducing material consumption, and further improving the lightweight effect.

[0034] (3) The present invention fully considers that when the Sn element is too little, it cannot play its beneficial role; when it is too much, it cannot be fully dissolved back into the matrix, resulting in performance deterioration. Therefore, the content of the Sn element is strictly controlled. In addition, the present invention fully considers that when the Cu element is too little, it cannot play its beneficial role; when it is too much, it will lead to increased strength and decreased stamping performance of the T4P state sheet, as well as decreased corrosion performance of the sheet. Therefore, the content of the Cu element is strictly limited.

[0035] (4) The present invention adopts a process without intermediate annealing to prepare 6xxx alloy plates, which has a short process and is conducive to industrial production scheduling; in addition, it has less carbon emissions and is more beneficial to environmental protection; the cost is low, which is conducive to market promotion. DETAILED DESCRIPTION

[0036] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0037] Terminology explanation:

[0038] Weight percentage: The percentage of a certain alloy component's mass (weight) to the total mass.

[0039] Yield strength: The yield limit of aluminum alloy when yielding occurs. The stress value that produces 0.2% residual deformation is defined as its yield limit. The stress-strain curve is obtained through uniaxial tensile test, and the yield strength data is obtained through the curve.

[0040] Yield strength in T4P state: The finished plate is obtained after melting, homogenization, hot rolling, cold rolling, solution treatment, pre-aging and slicing. After the finished plate is stored at room temperature for 7 days, the yield strength is obtained by testing the mechanical properties through a uniaxial tensile test.

[0041] Yield strength in T8X state: After the finished plate is stored at room temperature for 7 days, it is pre-stretched by 2% by a uniaxial stretching machine, and then kept in an oil bath furnace at 185℃ for 20 minutes to simulate the baking process in the actual production process of the OEM. The yield strength in the baking state is tested by a uniaxial tensile test.

[0042] Paint baking increment: the difference between the yield strength after baking and the yield strength in the initial state.

[0043] In the application, high stability means: the 7-day yield strength of T4P state plate is less than 100MPa, and the yield strength increment from 7 days to 180 days is less than 25MPa.

[0044] High baking hardening performance: T4P state sheet is pre-stretched by 2% and baked at 185℃ for 20min to obtain T8X state sheet, with yield strength greater than 200MPa and paint increment greater than 130MPa.

[0045] After the 6xxx aluminum alloy sheet is treated by solid solution pre-aging and other treatments at the aluminum processing plant, it is prepared into T4P state sheet and sent to the stamping plant for further stamping. In the T4P state, the sheet needs to have a lower yield strength to meet the requirements of stamping. In addition, since the 6xxx aluminum alloy has the characteristics of natural aging, the strength of the sheet will increase with the extension of the parking time, resulting in the deterioration of the forming performance. Therefore, it is necessary to suppress the occurrence of natural aging to ensure that the performance of the sheet is stable and meets the forming requirements. After the sheet is stamped, it will be painted. The 6xxx aluminum alloy sheet has the characteristics of heat treatment and strengthening. During the high-temperature treatment process of drying the paint, the strength of the sheet can be greatly improved, thereby meeting the requirements for strength performance.

[0046] At room temperature, Sn has a stronger vacancy binding ability than the main alloying elements Mg and Si in 6xxx alloys, so it can more effectively bind vacancies and inhibit the diffusion of Mg and Si elements, thereby greatly improving the room temperature parking stability of the board. When baked at high temperature, the vacancies will be released again, thereby improving the paint performance. Cu element can further improve the paint performance during the baking process.

[0047] Based on this, the present invention proposes the following technical solutions.

[0048] According to a typical embodiment of the present invention, an aluminum alloy plate with high stability and high bake hardening performance is provided. The aluminum alloy plate comprises the following components by mass percentage: Si: 0.20% to 1.50%; Fe: ≤0.40%; Cu: 0.06-0.30%; Mn: 0.05% to 0.2%; Mg: 0.20% to 0.80%; Cr: ≤0.10%; Ti: 0.01-0.05; Sn: 0.005-0.045%, and the balance Al.

[0049] The present invention adds trace Sn and Cu elements in combination, which not only effectively utilizes the characteristics of Sn elements to restrain vacancies and inhibit natural aging, but also combines the characteristics of Cu elements to improve the performance of baking varnish. Compared with the single addition of a certain alloy element, the performance of the sheet is further optimized. By adding trace Sn elements, compared with the main alloying elements Mg and Si in the 6xxx alloy, the Sn element has a stronger vacancy binding ability, thereby restraining vacancies, inhibiting the diffusion of Mg and Si elements, and greatly improving the room temperature parking stability of the sheet. And it is utilized to release the vacancies again during high-temperature baking, thereby improving the performance of baking varnish. By adding trace Cu elements, the characteristics of improving the strengthening effect of baking varnish during high-temperature baking are utilized to further improve the performance of baking varnish.

[0050] Moreover, the present invention can significantly improve the stability and paint performance by adding only a very small amount of Sn and Cu elements, without adding a large amount of Zn, Cu or expensive elements such as Sc and Zr as described in other patents, and the cost is controllable.

[0051] According to a typical embodiment of the present invention, an aluminum alloy plate is prepared by the following preparation method: (1) casting an aluminum alloy melt into an ingot; (2) subjecting the ingot to a homogenization treatment; (3) sequentially hot rolling and cold rolling the homogenized ingot to prepare a cold-rolled coil; (4) subjecting the cold-rolled coil to a solution treatment and a quenching treatment to obtain a coil; (5) subjecting the quenched coil to a pre-aging treatment to obtain a T4P state coil; (7) uncoiling, straightening, and slicing the T4P state coil after the pre-aging treatment to obtain an aluminum alloy plate.

[0052] The present invention does not require additional steps or equipment and can meet the requirements of industrial preparation.

[0053] Preferably, the homogenization treatment in step (2) is to heat up to 480-520°C at a rate of 40-70°C / h and keep warm for 4-10h, and then heat up to 560-580°C at a rate of 20-40°C / h and keep warm for 6-10h. In other words, the present invention adopts two-stage homogenization, on the one hand to ensure the effective dissolution of the Sn element, and on the other hand to fully consider the actual industrial production. The use of slow heating fully considers that the equipment capacity is limited during industrial production and rapid heating cannot be achieved. The purpose of the first stage homogenization is to promote the dissolution of the low-melting point phase, increase its melting point and thus increase the temperature of the second stage homogenization. The second stage homogenization temperature needs to reach above 560°C in order to ensure that the Sn element is more fully dissolved and solve the problem of low solubility of the Sn element in aluminum. However, when the temperature is too high, it will cause the material to be overburned and scrapped, so the temperature is controlled within the above range.

[0054] Preferably, the hot rolling start temperature in step (3) is 560-580°C, and the thickness of the hot rolled sheet is 4-8 mm. Under such conditions, the homogenization temperature and hot rolling temperature of the alloy are higher than those of conventional 6xxx alloys, and the effect of Sn can be fully exerted. Preferably, the thickness of the sheet after hot rolling and cold rolling in step (3) is 0.5-3.0 mm;

[0055] In a preferred embodiment of the present application, the solution treatment of step (4) is completed in an air cushion continuous annealing furnace, the temperature is raised to 565-585°C at a rate of more than 5°C / s, and the temperature is kept for 0.5-5min, and the temperature is cooled to room temperature at a rate of more than 30°C / s; the present invention adopts a high temperature solution temperature to ensure that the Sn element is more fully dissolved, thereby effectively utilizing the characteristics of the Sn element. However, when the temperature is too high, the material will be overburned and scrapped, so the temperature is controlled within the above range.

[0056] Preferably, the pre-aging treatment in step (5) is carried out in a box furnace at 60-90°C for 4-10 hours. A certain number of clusters will be precipitated during the pre-aging process, the purpose of which is: 1) consuming solutes and vacancies, thereby inhibiting natural aging and improving room temperature parking stability; 2) the precipitated clusters can be directly converted into a reinforcing phase during the paint baking, thereby improving the paint baking strength.

[0057] Preferably, the aluminum alloy sheet: the 7-day yield strength of the T4P state sheet is less than 100 MPa, and the yield strength increment from 7 days to 180 days is less than 25 MPa. The T4P state sheet is pre-stretched by 2% + baked at 185℃ for 20 minutes to obtain the T8X state sheet, the yield strength is greater than 200 MPa, and the baking paint increment is greater than 130 MPa.

[0058] The present invention is further supplemented and illustrated below in conjunction with specific implementation schemes. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of them.

[0059] Example

[0060] First, pure aluminum and various intermediate alloys are melted according to the composition ratio shown in Table 1. After the melt is refined, an ingot is cast using a semi-continuous casting device. After the ingot is cut and milled, it is placed in a heat treatment furnace for homogenization. After the homogenization treatment, the ingot is directly taken out of the furnace for hot rolling; after the hot rolling is completed, the obtained hot-rolled plate is cold-rolled; the obtained cold-rolled plate is uncoiled, straightened, and sliced ​​after solid solution, quenching, and pre-aging treatment to obtain a T4P state finished plate. Specific experimental parameters in the embodiment are shown in Table 2. In addition, in the following embodiments, if not specifically stated, the hot rolling start temperature in step (3) is 570°C, the hot-rolled plate thickness is 6mm, and the plate thickness after the hot rolling in step (3) is 2.0mm; the pre-aging treatment in step (5) is kept in a box furnace at 80°C for 6h.

[0061] Table 1 Composition of aluminum alloy sheets with high stability and high bake hardening performance

[0062]

[0063] Table 2 Preparation process of aluminum alloy sheets with high stability and high bake hardening performance

[0064]

[0065]

[0066] The mechanical properties of the finished plates in T4P state were tested after being stored at room temperature for 7 days and 180 days. The baking performance adopts the evaluation standard of most OEMs, that is, the finished plates are pre-stretched by 2%, then kept in an oil bath furnace at 185℃ for 20 minutes, and then quenched with water to room temperature before testing the mechanical properties. The mechanical properties are tested in accordance with "GB / T 13239-2006 Low Temperature Tensile Test Method for Metallic Materials".

[0067] Table 3 Mechanical properties of high-baked 6xxx aluminum alloy sheets (MPa)

[0068]

[0069]

[0070] Examples 1-2, Comparative Examples 1-2: According to 1 in Table 1 # Aluminum alloy composition preparation examples 1-2, corresponding to alloy numbers 1-1, 1-2, and comparative examples 1-2, corresponding to alloy numbers 1-3, 1-4, their preparation processes are shown in Table 2, and the mechanical properties of the final finished plates are shown in Table 3. The mechanical properties of the finished plates obtained in examples 1-2 are qualified. The mechanical properties of the plates obtained in comparative examples 1-2 are unqualified. The homogenization temperature of comparative example 1 is too low, and the Sn element fails to completely dissolve back and does not play its due role, resulting in poor room temperature stability of the T4P state plate and insufficient paint strength of the T8X state plate; the pre-aging temperature of comparative example 2 is too high, and the strength of the T4P state plate is too high, which is not conducive to stamping.

[0071] Examples 3-4, Comparative Example 3: According to 2 in Table 1 # Aluminum alloy composition preparation examples 3-4, corresponding to alloy numbers 2-1, 2-2, and comparative example 3, corresponding to alloy number 2-3, their preparation processes are shown in Table 2, and the mechanical properties of the final finished plates are shown in Table 3. The mechanical properties of the finished plates obtained in examples 3-4 are qualified. The mechanical properties of the finished plate obtained in comparative example 3 are unqualified. The homogenization temperature in comparative example 3 is too high, resulting in overburning and the material is scrapped.

[0072] Examples 5-6, Comparative Example 4: According to 3 in Table 1 # Aluminum alloy composition preparation examples 5-6, corresponding to alloy numbers 3-1, 3-2, and comparative example 4, corresponding to alloy number 3-3, the preparation process is shown in Table 2, and the mechanical properties of the final finished plate are shown in Table 3. The mechanical properties of the finished plates obtained in Examples 5-6 are qualified. The mechanical properties of the finished plate obtained in Comparative Example 4 are unqualified. The solid solution temperature of Comparative Example 4 is too low, and the Sn element fails to completely dissolve back and does not play its due role, resulting in poor room temperature stability of the T4P state plate and insufficient paint strength of the T8X state plate.

[0073] Examples 7-8, Comparative Example 5: According to 4 in Table 1 # Aluminum alloy composition preparation examples 7-8, corresponding to alloy numbers 4-1, 4-2, and comparative example 5, corresponding to alloy number 4-3, their preparation processes are shown in Table 2, and the mechanical properties of the final finished plates are shown in Table 3. The mechanical properties of the finished plates obtained in examples 3-4 are qualified. The mechanical properties of the finished plate obtained in comparative example 5 are unqualified. The solution temperature of comparative example 5 is too high, resulting in overburning, and the material is scrapped.

[0074] Comparative Example 6: According to 5 in Table 1 # Aluminum alloy composition preparation Comparative Example 6 corresponds to alloy No. 5-1, and its preparation process is shown in Table 2, and the mechanical properties of the final finished plate are shown in Table 3. The mechanical properties of the finished plate obtained in Comparative Example 6 are unqualified. In Comparative Example 6, insufficient Sn and Cu elements are added, resulting in insufficient room temperature parking stability in the T4P state and insufficient baking paint strength in the T8X state.

[0075] Comparative Example 7: According to 6 in Table 1 # Aluminum alloy composition preparation comparative example 7 corresponds to alloy number 6-1, its preparation process is shown in Table 2, and the mechanical properties of the final finished plate are shown in Table 3. The mechanical properties of the finished plate obtained in comparative example 7 are unqualified. The content of Cu and Sn elements in comparative example 7 is too high, resulting in too high yield strength of the plate in the T4P state.

[0076] Comparative Example 8: According to 7 in Table 1 # Aluminum alloy composition preparation comparative example 8, corresponding to alloy number 7-1, its preparation process is shown in Table 2, and the mechanical properties of the final finished plate are shown in Table 3. The mechanical properties of the finished plate obtained in comparative example 7 are unqualified. The Cu element in comparative example 7 is too low, and the baking paint increment is insufficient.

[0077] Comparative Example 9: According to 8 in Table 1 # Aluminum alloy composition preparation comparative example 9, corresponding to alloy number 8-1, its preparation process is shown in Table 2, and the mechanical properties of the final finished plate are shown in Table 3. The mechanical properties of the finished plate obtained in comparative example 7 are unqualified. The Sn element in comparative example 7 is too low, the room temperature parking stability is insufficient, and the baking paint increment is insufficient.

[0078] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0079] (1) The present invention can achieve a low yield strength and stable performance in the T4P state of the sheet by adding trace amounts of Sn and Cu elements, greatly improving its stamping forming performance and meeting the forming requirements of more complex parts;

[0080] (2) The present invention can achieve higher paint performance after the board is baked by adding trace amounts of Sn and Cu elements, thereby achieving material thinning under equal strength, reducing material consumption, and further improving the lightweight effect;

[0081] (3) The present invention fully considers that when the Sn element is too little, it cannot play its beneficial role; when it is too much, it cannot be fully dissolved back into the matrix, resulting in performance deterioration. Therefore, the content of the Sn element is strictly controlled. In addition, the present invention fully considers that when the Cu element is too little, it cannot play its beneficial role; when it is too much, it will lead to increased strength and decreased stamping performance of the T4P state sheet, as well as decreased corrosion performance of the sheet. Therefore, the content of the Cu element is strictly limited;

[0082] (4) The present invention adopts a process without intermediate annealing to prepare 6xxx alloy plates, which has a short process and is conducive to industrial production scheduling; in addition, it has less carbon emissions and is more beneficial to environmental protection; the cost is low, which is conducive to market promotion.

[0083] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A high stability, high bake hardening performance aluminum alloy sheet, It is characterized in that The aluminum alloy plate comprises the following components by mass percentage: Si: 0.20% to 1.50%; Fe: ≤0.40%; Cu: 0.06-0.30%; Mn: 0.05% to 0.2%; Mg: 0.20%~0.80%; Cr: ≤0.10%; Ti: 0.01-0.05; Sn: 0.005-0.045%, and the balance is Al.

2. The aluminum alloy sheet according to claim 1, It is characterized in that The aluminum alloy sheet is prepared by the following preparation method: (1) casting an aluminum alloy melt into an ingot; (2) performing a homogenization treatment on the ingot; (3) hot rolling and cold rolling the homogenized ingot in sequence to prepare a cold-rolled coil; (4) performing solution treatment and quenching treatment on the cold-rolled coil to obtain a coil; (5) performing a pre-aging treatment on the quenched coil to obtain a T4P state coil; (7) Uncoiling, straightening, and slicing the T4P state coil after pre-aging treatment to obtain the aluminum alloy plate.

3. The aluminum alloy sheet according to claim 2, It is characterized in that The homogenization treatment in step (2) is to heat the mixture to 480-520°C at a rate of 40-70°C / h and keep the temperature for 4-10h, and then heat the mixture to 560-580°C at a rate of 20-40°C / h and keep the temperature for 6-10h.

4. The aluminum alloy sheet according to claim 2, It is characterized in that The hot rolling start temperature in step (3) is 560-580° C., and the thickness of the hot rolled plate is 4-8 mm.

5. The aluminum alloy sheet according to claim 2, It is characterized in that The thickness of the plate after hot rolling and cold rolling in step (3) is 0.5-3.0 mm.

6. The aluminum alloy sheet according to claim 2, It is characterized in that The solution treatment in step (4) is performed in an air cushion continuous annealing furnace, where the temperature is raised to 565-585°C at a rate of more than 5°C / s, kept at that temperature for 0.5-5 min, and then cooled to room temperature at a rate of more than 30°C / s.

7. The aluminum alloy sheet according to claim 2, It is characterized in that The pre-aging treatment in step (5) is carried out in a box-type furnace at 60-90° C. for 4-10 hours.

8. The aluminum alloy sheet according to any one of claims 1 to 7, It is characterized in that The aluminum alloy sheet material: the 7-day yield strength of the T4P state sheet material is less than 100MPa, and the yield strength increment from 7 days to 180 days is less than 25MPa. The T4P state sheet material is subjected to 2% pre-stretching + baking at 185°C for 20 minutes to obtain the T8X state sheet material, the yield strength of which is greater than 200MPa, and the baking paint increment is greater than 130MPa.

9. Use of the aluminum alloy sheet with high stability and high bake hardening performance as claimed in any one of claims 1 to 8 in automobile manufacturing.

10. A method for preparing an aluminum alloy sheet with high stability and high bake hardening performance, It is characterized in that include: (1) casting an aluminum alloy melt into an ingot; (2) performing a homogenization treatment on the ingot; (3) hot rolling and cold rolling the homogenized ingot in sequence to prepare a cold-rolled coil; (4) performing solution treatment and quenching treatment on the cold-rolled coil to obtain a coil; (5) performing a pre-aging treatment on the quenched coil to obtain a T4P state coil; (7) uncoiling, straightening, and slicing the T4P state coil after pre-aging treatment to obtain the aluminum alloy plate; The aluminum alloy plate comprises the following components by mass percentage: Si: 0.20% to 1.50%; Fe: ≤0.40%; Cu: 0.06-0.30%; Mn: 0.05% to 0.2%; Mg: 0.20% to 0.80%; Cr: ≤0.10%; Ti: 0.01-0.05; Sn: 0.005-0.045%, and the balance Al.

Citation Information

Cited By

  • Aluminum alloy sheet having high stability and high baking hardening performance, preparation method therefor and use thereof

    WO2026012250A1